A molecular sieve with transition metal atom pre-occupancy and secondary hydrothermal isomorphous substitution, and preparation method and application thereof
The MFI molecular sieve prepared by the transition metal atom pre-occupancy-secondary hydrothermal isomorphous substitution method solves the problems of high energy consumption and insufficient material selectivity in the process of improving the purity of ethylene gas in the existing technology, and achieves low-concentration ethane Preferential adsorption and efficient separation, suitable for chemical industry.
Patent Information
- Application Number
- CN202310309533.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-03-28
AI Technical Summary
The existing technology consumes high energy and is expensive in the process of improving the purity of ethylene gas, and the existing porous materials have insufficient selectivity and stability in ethane-ethylene separation, making it difficult to achieve preferential adsorption of low-concentration ethane.
The preparation method of MFI molecular sieves adopts the pre-occupancy of transition metal atoms and secondary hydrothermal isomorphous substitution. Zinc atoms occupy the skeleton positions in the pre-hydrothermal synthesis, and then isomorphous substitution species are added to realize the replacement of zinc atoms in the molecular sieve skeleton. Concentration substitution, regulating the electrostatic field and pore size, optimizing the adsorption performance of ethane.
It achieves preferential adsorption of low-concentration ethane in high-concentration ethylene gas, reduces energy consumption, improves separation selectivity and uniformity of active site distribution, and is suitable for adsorption catalytic reactions in the chemical industry.
Smart Images

Figure CN116477637B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a transition metal atom pre-occupancy-secondary hydrothermal isomorphous substitution molecular sieve and a preparation method and application thereof. The molecular sieve can efficiently adsorb trace ethane gas in high-purity polymerization-grade ethylene gas, and belongs to the field of gas adsorption separation. Background Art
[0002] Ethylene is an important petrochemical product, with an annual output of up to 100 million tons, and it occupies an important position among all petrochemical products. The industrial preparation of ethylene is usually produced by high-temperature cracking of ethane, but the final product is often a mixture of a small amount of ethane and a large amount of ethylene. In order to further improve the purity of ethylene gas, the industry often uses a deep cold separation method to further separate and purify the product mixed gas after cracking. However, this process consumes a lot of energy, has high production costs, and is not economically efficient (Nat. Commun., 2015, 6, 8697). The existing low-energy purification methods for ethylene include absorption separation, membrane separation, and pressure swing adsorption technology. The absorption separation method needs to introduce a certain amount of absorbent during the absorption process, and the mixed gas is controlled to only perform one-way mass transfer of the gas phase-liquid phase. It is also necessary to perform analytical operations to recover the absorbent therein. Patent CN103058810A reports a suspension slurry with a metal-organic framework for ethane and ethylene separation. The separation equipment involved in this method is numerous and costly, and the suspension slurry still needs to be analyzed in the later stage. The membrane separation method uses the difference in molecular size and diffusion performance between ethane and ethylene, but the molecular size difference between ethane and ethylene is small, and the membrane material is expensive and easy to damage. The higher the selectivity of the membrane, the worse the gas permeability. Pressure swing adsorption technology can achieve effective separation of low-concentration gases at room temperature, thereby solving the high energy consumption problem of traditional methods.
[0003] Porous materials have been widely studied as solid adsorbents commonly used in pressure swing adsorption technology. Currently, commonly used porous materials mainly include carbon materials, metal organic framework materials (MOFs) and zeolite molecular sieves. In the process of ethane and ethylene separation, the material needs to have high separation selectivity, while carbon materials are often widely adsorbed in the gas adsorption process and cannot achieve the product purity required in the industry. MOFs is a three-dimensional network structure formed by cross-linking metal nodes and organic ligands, which usually has a uniform pore size of 0.3nm-2nm (Nature, 2003, 423, 705). Although there are reports on the adsorption and separation of ethane-ethylene mixed gases by MOFs materials, ethylene is usually adsorbed in large quantities first, and the energy consumption of adsorption and separation in high-concentration ethylene systems is relatively high (J.Am.Chem.Soc.2021,143,8654-8660). Patent CN105709693A reports the application of a flexible MOFs material in ethane-ethylene adsorption separation, which preferentially adsorbs ethylene gas in large quantities. Although Li et al. will contain Fe(Ⅲ)-O2 2- The MOF-47 with the site is applied to ethane and ethylene separation, and can preferentially and selectively adsorb ethane gas therein, but the reported ethane-ethylene adsorption capacity ratio is only 1.25, and the adsorption separation performance is still poor (Science, 2018, 362, 443–446). In addition, patent CN105949028 reports a special MOFs material preparation method, which preferentially adsorbs oxygen molecules at the unsaturated sites of the material, limits the interaction between the unsaturated sites and ethylene molecules, and makes it well applied in ethane separation, but the ethane separation selectivity will decrease significantly with the decrease of concentration. In addition, the MOFs material itself has poor hydrothermal stability, which limits its application in industry. Zeolite molecular sieves are often used in the separation process of different gas components in mixed gases. Its basic structure is a ring structure formed by regular tetrahedrons centered on Si atoms or Al atoms connected by oxygen bridges. The advantages of zeolite molecular sieves are stable structure, uniform and adjustable pores, and good recycling and regeneration performance during gas separation. At present, the zeolite molecular sieves with better ethane and ethylene separation effects are ITQ-55 molecular sieve, LTA type, FAU type and ETS type molecular sieve. However, due to the stronger polarity of ethylene gas, most of the current molecular sieves used in ethane and ethylene separation studies have preferentially adsorbed the ethylene component, and later thermal desorption is required to obtain high-purity ethylene gas (J.Am.Chem.Soc.2012,134,14635-14637). MFI molecular sieve is a small-pore molecular sieve with a main pore composed of ten-membered rings and a pore size of The pore size of MFI molecular sieve matches the size of ethane and ethylene gas molecules, and the pore size of MFI molecular sieve and the size of ethane molecules The pore wall adsorption is stronger, which makes it very suitable for the separation of low-concentration ethane. However, there are still few reports on the application of MFI molecular sieves in ethane and ethylene adsorption separation processes.
[0004] At present, the adsorption and separation effect of molecular sieves is mainly achieved by introducing active metals to regulate the electrostatic adsorption force. The control methods of electrostatic action mainly include impregnation, ion exchange, and isomorphous substitution. Among them, impregnation is mainly physical mixing, and active metal species are difficult to enter the molecular sieve framework. Patent CN114477205A reports a process of preparing titanium-containing MFI molecular sieves using an impregnation method. The obtained sample is only rich in titanium species on the surface of the molecular sieve. Patent CN108187607A reports a method of using equal volume impregnation to dope metal active salt active components in titanium silicon molecular sieves for application in ethane ethylene adsorption separation process. The ethylene ethane adsorption separation factor is 6.57, and the adsorption amount of ethylene by the adsorption separation agent is 2.602mmol / g, and the adsorption amount of ethane is 0.396mmol / g, which still cannot achieve preferential separation of ethane. Introducing heteroatoms into molecular sieves through ion exchange easily leads to strong electrostatic fields. Patent CN104549141A selects lanthanide metal elements to modify molecular sieve materials through ion exchange, showing extremely strong polarity and induction in the molecular sieve framework. The same patent CN111747819B uses imidazole compounds to modify MFI molecular sieves through ion exchange and applies them to ethane-ethylene separation, with an equilibrium separation ratio of only 1.1. In the ethane-ethylene separation process, due to the weak polarity of ethane, the preferential adsorption and separation of ethane requires the use of weakly polar molecular sieve materials, so the ion exchange method is not suitable for preferentially capturing low-concentration ethane gas in the mixed gas. Relatively speaking, the isomorphous substitution method can more easily obtain a relatively weak electrostatic field while introducing active metal sites compared to the previous two methods, and has more advantages in regulating the adsorption and separation force of low-concentration ethane.
[0005] The isomorphous substitution method mainly utilizes the substitution of heteroatoms with framework atoms under certain driving force conditions during the hydrothermal crystallization process to synthesize a molecular sieve with a high framework heteroatom ratio. Patent CN109513458B reports a one-step hydrothermal crystallization method for synthesizing an MFI molecular sieve containing tungsten atoms in the framework, but the molecular sieve synthesized by this method has an extremely low tungsten atom content in the framework, and has fewer adsorption and catalytic active sites. Patent CN113307285A proposes to first hydrothermally form a silicon-containing precursor, and then add a water-soluble inorganic salt or organic compound containing heteroatoms to continue crystallization to obtain a heteroatom-doped molecular sieve, but because Si atoms are extremely stable in the molecular sieve framework, heteroatoms can only replace a small amount of molecular sieve framework sites, and the adsorption catalytic performance is not high. Patent CN 111229301 A proposes adding Fe simultaneously during the hydrothermal crystallization process of the MFI molecular sieve. 3+ Ion, Fe 3+Will replace some Al 3+ The ions enter the molecular sieve framework to generate Fe-MFI molecular sieve, thereby changing the physical and chemical properties of the molecular sieve itself. However, the above methods all use a one-step method to achieve isomorphous substitution of active metals, which cannot achieve accurate substitution of metal atoms and fine regulation of the electrostatic field effect, and some metal atoms cannot achieve isomorphous substitution of framework atoms by a one-step method. Therefore, it is urgent to further develop a new molecular sieve synthesis method that can control the electrostatic field of molecular sieves by isomorphous substitution of active metals.
[0006] Given that active metals easily occupy specific molecular sieve structural sites during the hydrothermal synthesis of molecular sieves, especially zinc atoms, which are easy to settle in the molecular sieve framework to form active metal sites, and are very easy to remove in subsequent experiments without causing changes in the molecular sieve framework structure (Dalton Trans., 2018, 47, 15082–15090). At the same time, it has been reported that there is a reversible bonding-breaking process between the framework T atoms and oxygen atoms during the hydrothermal process (Angew. Chem. Int. Ed. 2020, 59, 20672–20681). Therefore, based on the above phenomenon, this paper proposes a new method for preparing MFI zeolite by pre-occupation of transition metal atoms and secondary hydrothermal isomorphous substitution. Zinc atoms are used to preferentially occupy specific sites in the framework during the pre-hydrothermal synthesis of the zeolite, and then high-concentration isomorphous substitution species are added during the secondary crystallization process. The concentration difference substitution of zinc atoms in the zeolite framework by isomorphous substitution metal species is used to achieve the directional substitution of active metals on the framework sites and the fine control of the electrostatic field on the surface of the zeolite, thereby achieving the preferential adsorption of low-concentration ethane in a large amount of ethylene. Summary of the invention
[0007] In view of the above-mentioned technical problems existing in the prior art, the object of the present invention is to provide a method for preparing a molecular sieve with transition metal atom pre-occupancy and secondary hydrothermal isomorphous substitution and its application. The present invention relates to an MFI molecular sieve adsorbent with transition metal atom pre-occupancy and secondary hydrothermal isomorphous substitution, which can efficiently capture low-content ethane gas.
[0008] To achieve the above purpose, the present invention adopts tetrapropylammonium hydroxide as the alkaline template of the hydrothermal system, promotes the large-scale and stable entry of heteroatoms into the molecular sieve framework by optimizing the experimental method, and successfully synthesizes MFI molecular sieves with high silicon content, which preferentially adsorb ethane and is suitable for use as an adsorbent for the adsorption and separation of low-content ethane-high-content ethylene gas systems.
[0009] The technical solution adopted by the present invention is as follows:
[0010] The invention discloses a molecular sieve with transition metal atom pre-occupancy and secondary hydrothermal isomorphous substitution. The preparation method of the molecular sieve adopts zinc atoms to occupy specific skeleton positions in the preliminary hydrothermal synthesis, washes and roasts after the crystal is stable, and then mixes with W isomorphous substitution raw materials, alkaline template and water, and performs secondary hydrothermal synthesis to realize isomorphous substitution. The chemical composition molar ratio of the obtained molecular sieve product is aYO2:bZnO:cH2O:dWOx, wherein 10≤a≤40, 0.025≤b≤1, 0<c≤11, 0.0125≤d≤1, Y is a tetravalent element, W is an isomorphous substitution element after the crystal is stable, and when measured by X-ray diffraction, the molecular sieve has characteristic peaks within at least the following four crystal plane spacings (d), the first crystal plane spacing d=11.0±0.3, the second crystal plane spacing d=9.9±0.2, the third crystal plane spacing d=4.3±0.2, and the fourth crystal plane spacing d=3.8±0.2.
[0011] Furthermore, the transition metal atom pre-occupied and secondary hydrothermal isomorphously substituted molecular sieve has an MFI molecular sieve configuration recognized by the International Zeolite Association (IZA); the element composition contains a relatively large amount of tetravalent element Y, and relatively small amounts of divalent transition metal element zinc and isomorphously substituted metal element W, and as determined by inductively coupled plasma spectroscopy, 10≤a≤20, 0.05≤b≤0.4, 0<c≤2.5, 0.05≤d≤0.1.
[0012] Furthermore, in the molecular sieve with transition metal atom pre-occupancy and secondary hydrothermal isomorphous substitution, Y in the chemical composition is a tetravalent element, including one or more of Si, Ge, and Sn elements, preferably Si; W in the chemical composition is an isomorphous substitution element, including but not limited to Ni, Mn, Cu, Ti, Sn and other elements.
[0013] The method for preparing a transition metal atom pre-occupied molecular sieve with secondary hydrothermal isomorphous substitution is carried out according to the following steps: a precursor gel solution is formed by mixing aqueous solutions of compound raw materials containing at least an alkaline template, zinc acetate and a tetravalent element Y, and a solid-liquid mixture of a molecular sieve doped with a metal zinc skeleton is obtained after a hydrothermal synthesis reaction; the molecular sieve solid-liquid mixture is then centrifuged, washed, and dried, and then placed in an air atmosphere for high-temperature calcination, and then the obtained solid powder, alkaline template, W isomorphous substitution raw material and water are mixed and stirred uniformly, and secondary hydrothermal synthesis is continued, and isomorphous substitution is achieved by concentration difference substitution of high-concentration W element for zinc element in the molecular sieve skeleton to obtain a new solid-liquid mixture of metal atom isomorphous substitution molecular sieve, and then the pre-occupied molecular sieve with secondary hydrothermal isomorphous substitution is obtained through centrifugation, washing, drying and roasting.
[0014] The specific steps of preparing the molecular sieve of the present invention are as follows:
[0015] (a) adding alkaline template agent tetrapropylammonium hydroxide and deionized water to a reaction kettle in sequence, heating and stirring to fully dissolve and mix them, then adding zinc acetate and compound raw materials containing tetravalent element Y in the above molecular sieve composition according to the oxide molar ratio of (10-40)YO2:ZnO, stirring and aging to obtain an initial gel solution, transferring it to a closed reaction kettle for hydrothermal synthesis reaction, and obtaining a molecular sieve solid-liquid mixture in which zinc atoms occupy specific skeleton positions;
[0016] (b) centrifuging, washing, drying, grinding, and then calcining and activating the molecular sieve solid-liquid mixture after the reaction in step (a) to remove organic matter in the molecular sieve solid-liquid mixture to obtain a solid powder;
[0017] (c) the solid powder obtained in step (b), alkaline template agent tetrapropylammonium hydroxide, W isomorphous substitution raw material and water are uniformly stirred, and secondary hydrothermal crystallization is continued to achieve isomorphous substitution by concentration difference substitution of high concentration W element on the zinc element in the molecular sieve framework, and then centrifuged, washed, dried and calcined to obtain the solid-liquid mixture of the molecular sieve.
[0018] In the chemical composition of the MFI molecular sieve in step (a), Y is a tetravalent element, including but not limited to one or more of Si, Ge, Sn and the like, preferably Si, Sn, more preferably Si, and the corresponding silicon source includes one or a mixture of silica sol, silica gel, active silica or orthosilicate.
[0019] Further optimization, in step (a), the molar ratio of zinc acetate and the oxide of the compound raw material containing the tetravalent element Y is (20-30) YO2: ZnO. In step (a), the mass ratio of deionized water to tetrapropylammonium hydroxide is 2-6:1, preferably 3-3.5:1; the mass ratio of the template agent tetrapropylammonium hydroxide to the tetravalent element Y compound raw material is 25-30%, preferably 25%.
[0020] Further optimization, the aging time in step (a) is preferably 12h-16h, the aging temperature is selected to be room temperature, and during the aging process, wind blowing, heating and other methods are added to remove the volatile alcohol components in the tetravalent element Y compound raw material. The reaction temperature of hydrothermal crystallization is 180-220°C, most preferably 200°C, and the reaction time of hydrothermal synthesis is the molecular sieve crystallization stability time, which is selected to be 2.8-3.2h, preferably 3h.
[0021] Further optimization, in step (b), the drying process temperature is selected to be 60-150°C, preferably 80-120°C, and the drying time is selected to be 2-24h. The dried molecular sieve solid sample needs to be heated and calcined to remove the internal template agent so that it has adsorption and catalytic properties. The calcination temperature is selected to be 400-700°C, preferably 500-600°C, and the constant temperature calcination time is selected to be 2-12h, preferably 3-8h, and more preferably 4-7h.
[0022] Further optimization, in step (c), the stirring mixing time is selected to be 0.1-1h, preferably 0.5-1h, the stirring temperature is selected to be 10-50°C, preferably 20-30°C, the crystallization temperature in step (c) is the same as the hydrothermal synthesis temperature in step (a), the crystallization temperature is 180-220°C, preferably 200°C, the crystallization time is selected to be 1-8h, preferably 2-6h, and more preferably 4-5h; the calcination temperature and time in step (c) are the same as those in step (b), the calcination temperature in step (c) is selected to be 400-700°C, preferably 500-600°C, and the calcination time is selected to be 2-12h, preferably 3-8h, and more preferably 4-7h.
[0023] The transition metal atom pre-occupied-secondary hydrothermal isomorphous substitution molecular sieve of the present invention can be used to selectively absorb and separate ethane in the atmosphere of an ethane-ethylene system to achieve the separation of ethane and ethylene. Compared with commercial silicon-aluminum molecular sieves and traditional one-step synthesized metal atom-doped molecular sieves, it can preferentially adsorb ethane in large quantities.
[0024] The transition metal atom pre-occupancy-secondary hydrothermal isomorphous substitution molecular sieve adsorption and separation of gas can be operated at 273-323K, preferably 288-308K.
[0025] The transition metal atom pre-occupancy-secondary hydrothermal isomorphous substitution molecular sieve of the present invention can be applied to the preferential selective adsorption separation of low-concentration ethane gas in a large amount of ethylene.
[0026] The present invention is a technical advancement compared to the prior art;
[0027] (1) The transition metal atom pre-occupancy-secondary hydrothermal isomorphous substitution molecular sieve in the present invention changes the molecular sieve pore size and surface polarity through precise regulation of the skeleton atomic sites, increases the recognition of ethane in the ethane-ethylene mixed gas by the adsorption sites, realizes the preferential selective adsorption and separation of ethane, effectively improves the preferential large-scale adsorption of traditional molecular sieves in low-concentration ethane systems, and reduces energy consumption.
[0028] (2) The method for synthesizing the transition metal pre-occupied-secondary hydrothermal isomorphous substitution molecular sieve of the present invention uses the concentration difference theorem to introduce isomorphous substitution elements when the crystallinity of hydrothermal synthesis is stable. Compared with the current one-step isomorphous substitution, more heteroatoms can be introduced into the framework, and the distribution of active metal sites in the obtained molecular sieve is more uniform. In addition, compared with impregnation and ion exchange, this method can obtain a relatively weak electrostatic field, which is more conducive to the adsorption and separation of weak polarity low-concentration ethane gas in ethane and ethylene mixed gas.
[0029] (3) By using the transition metal pre-occupancy-secondary hydrothermal isomorphous substitution molecular sieve preparation method of the present invention to replace different metal atoms into the molecular sieve framework, a molecular sieve with different active metal sites can be obtained, and then it is applied to various adsorption catalytic reactions according to the characteristics of the metal atoms themselves. Since most of the active sites exist in the framework, the molecular sieve after isomorphous substitution has high activity and excellent reproducibility. This preparation method provides some references for the development of porous materials in the chemical industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a schematic diagram of the XRD test results of H-MFI-Zn / 10 in Example 1;
[0031] Figure 2 is a schematic diagram of the XRD test results of H-MFI-Zn / 20 in Example 2;
[0032] Figure 3 is a schematic diagram of the crystallinity and solid yield curve of H-MFI-Zn / 20 in Example 2;
[0033] Figure 4 is a schematic diagram of the XRD test results of H-MFI-Zn / 30 in Example 3;
[0034] Figure 5 is a schematic diagram of the XRD test results of H-MFI-Zn / 40 in Example 4;
[0035] Figure 6 is a schematic diagram of the ethane gas adsorption curve of H-MFI-Zn in Examples 1, 2, 3, and 4;
[0036] Figure 7 is a schematic diagram of the XRD test results of H-MFI-Zn / 20+Sn in Example 5;
[0037] Figure 8 is a schematic diagram of the ethane ethylene breakthrough curve of H-MFI-Zn / 20+Sn in Example 5;
[0038] Fig. 9is a schematic diagram of the XRD test results of H-MFI-Zn / 20+Ti in Example 6;
[0039] Fig.10 is a schematic diagram of the ethane ethylene breakthrough curve of H-MFI-Zn / 20+Ti in Example 6;
[0040] Fig.11 is a schematic diagram of the XRD test results of H-MFI-Zn / 20+Mn in Example 7;
[0041] Fig.12 is a schematic diagram of the ethane ethylene breakthrough curve of H-MFI-Zn / 20+Mn in Example 7;
[0042] Fig.13 is a schematic diagram of the XRD test results of H-MFI-Zn / 20+Cu in Example 8;
[0043] Fig.14 This is a schematic diagram of the ethane ethylene breakthrough curve of H-MFI-Zn / 20+Cu in Example 8
[0044] Fig.15 is a schematic diagram of the XRD test results of H-MFI-Zn / 20+Ni in Example 9;
[0045] Fig.16 Schematic diagram of ethane ethylene breakthrough curve of H-MFI-Zn / 20+Ni in Example 9
[0046] Fig.17 This is a schematic diagram of the XRD test results of H-MFI-Sn / 20 in Comparative Example 1;
[0047] Fig.18 Schematic diagram of ethane ethylene breakthrough curve of H-MFI-Sn / 20 in comparative example 1
[0048] Fig.19 This is a schematic diagram of the XRD test results of H-MFI-Mn / 20 in Comparative Example 2;
[0049] Fig. 20 Schematic diagram of ethane ethylene breakthrough curve of H-MFI-Sn / 20 in comparative example 2
[0050] Fig.21 This is a schematic diagram of the ethane ethylene breakthrough curve of MFI-Al / 50 in Comparative Example 4; DETAILED DESCRIPTION
[0051] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0052] <Example 1>
[0053] 0.32g of deionized water was added to 6.8877g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6g of TEOS (mass percentage of about 98%) and 0.6258g of zinc acetate dihydrate (mass percentage of about 99%) were added in sequence, and the initial gel solution was obtained after aging at room temperature for 12 hours. The initial solution was added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and static crystallization was carried out at a reaction temperature of 200°C for 3 hours. After the hydrothermal reaction was completed, the reactor was cooled, the reaction solution was taken out and centrifuged, and the crystallized product was obtained by washing. The obtained crystals were dried at 110°C for 5h, ground, and calcined in air: heated to 580°C at a rate of 2°C / min, maintained at 580°C for 6h to fully volatilize the water and organic matter therein, and then cooled to 80°C to obtain H-MFI-Zn / 10 (the naming convention for all homemade molecular sieves is: H-MFI-Zn / 10, where H is the type of balanced cation, MFI is the molecular sieve configuration, Zn is the type of transition metal atom, and 10 is the molar ratio of silicon to transition metal atoms, the same below). The calcined sample was taken out and placed in a drying dish for storage. The obtained product was analyzed for product crystal phase by XRD. The interplanar spacing of the characteristic peaks in H-MFI-Zn / 10 is shown in Table 1. The schematic diagram of the XRD test results is shown in the figure. Figure 1 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0054] The above H-MFI-Zn / 10 was used for the adsorption of ethane or ethylene gas. The gas adsorption isotherm of the sample was measured on the adsorption instrument 3Flex of Micromeritics. The adsorbed gases were ethane (99.99%) and ethylene (99.99%). In order to study the effect of pre-occupied atoms doping the molecular sieve structure on the ethane adsorption effect, the above molecular sieve was dehydrated in 3Flex to avoid the effect of physically adsorbed water in the molecular sieve on the gas adsorption effect. Under low vacuum conditions (below 0.005 mmHg), it was heated to 100°C at a heating rate of 5°C / min, maintained for 1h, and then continued to heat to 200°C at a rate of 5°C / min, maintained for 1h, and then continued to heat to 350°C at a rate of 5°C / min, and maintained at 350°C for 6h. The sample tube was then placed in a 3Flex adsorption device for a static adsorption curve test (0-1 bar). A constant temperature water bath (accuracy 0.01°C) was used to control the temperature in the gas adsorption sample tube. The adsorption temperature was 298K. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 10 is shown in Table 12.
[0055] Table 1 Characteristic interplanar spacing of H-MFI-Zn10
[0056] Interplanar spacing (d) 1 11.141 2 9.992 3 6.710 4 4.365 5 4.003 6 3.846 7 3.756
[0057] Table 1 lists the interplanar spacings of the seven characteristic peaks in H-MFI-Zn / 10. The seven characteristic peaks correspond to Figure 1 The seven arrows in the figure point to characteristic peaks, the same below.
[0058] <Example 2>
[0059] 0.3713g of deionized water was added to 6.8877g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6g of TEOS (mass percentage of about 98%) and 0.3129g of zinc acetate dihydrate (mass percentage of about 98%) were added in sequence, and the initial gel solution was obtained after aging at room temperature for 12 hours. The initial solution was added to a stainless steel crystallization kettle with a polytetrafluoroethylene liner and sealed, and statically crystallized for 3 hours at a reaction temperature of 200°C and autogenous pressure (3 hours is the highest hydrothermal crystallization time of the transition metal-doped MFI molecular sieve sample, so it is used as the reaction time of the isomorphous substitution precursor. The schematic diagram of the crystallinity curve is shown in the figure. Figure 3 As shown). After the thermal reaction is completed, the reactor is cooled, the reaction solution is taken out, centrifuged, and washed to obtain a crystalline product. The obtained crystals are dried at 110°C for 5 hours, ground, and calcined in air: heated to 580°C at a rate of 2°C / min, maintained at 580°C for 6 hours to fully volatilize the moisture and organic matter therein, and then cooled to 80°C to obtain H-MFI-Zn / 20. The calcined sample is taken out and placed in a drying dish for storage. The obtained product is analyzed by XRD for product crystal phase. The interplanar spacing of the characteristic peaks in H-MFI-Zn / 20 is shown in Table 2. The schematic diagram of the XRD test results is shown in Figure 2 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0060] The above-mentioned H-MFI-Zn / 20 is used to adsorb ethane or ethylene gas. The adsorption test conditions are repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 20 is shown in Table 12.
[0061] Table 2 Characteristic interplanar spacing of H-MFI-Zn / 20
[0062] Interplanar spacing (d) 1 11.112 2 9.993 3 6.683 4 4.353 5 4.076 6 3.845 7 3.744
[0063] <Example 3>
[0064] The preparation method of H-MFI-Zn / 30 in Example 3 repeats the preparation process of H-MFI-Zn / 10 in Example 1, except that "the amount of zinc acetate dihydrate (mass percentage of about 98%) is replaced by 0.2065g from 0.6258g". The calcined sample is taken out and placed in a drying dish for storage. The obtained product is analyzed by XRD for product crystal phase. The interplanar spacing of characteristic peaks in H-MFI-Zn / 30 is shown in Table 3. The schematic diagram of XRD test results is shown in Figure 4 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0065] The above-mentioned H-MFI-Zn / 30 was used to adsorb ethane or ethylene gas. The adsorption test conditions were repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 30 is shown in Table 12.
[0066] Table 3 Characteristic interplanar spacing of NH-MFI-Zn / 30
[0067] Interplanar spacing (d) 1 11.138 2 10.001 3 5.981 4 4.362 5 4.002 6 3.843 7 3.756
[0068] <Example 4>
[0069] The preparation method of H-MFI-Zn / 40 in Example 4 repeats the preparation process of H-MFI-Zn / 10 in Example 1, except that "the amount of zinc acetate dihydrate (mass percentage of about 98%) is replaced by 0.1565g from 0.6258g". The calcined sample is taken out and placed in a drying dish for storage. The obtained product is analyzed by XRD for product crystal phase. The interplanar spacing of the characteristic peaks in H-MFI-Zn / 40 is shown in Table 4. The schematic diagram of the XRD test results is shown in Figure 5 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0070] The above-mentioned H-MFI-Zn / 40 is used to adsorb ethane or ethylene gas. The adsorption test conditions are repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 40 is shown in Table 12.
[0071] Table 4 Characteristic interplanar spacing of H-MFI-Zn / 40
[0072] Interplanar spacing (d) 1 11.076 2 9.951 3 5.962 4 4.355 5 3.993 6 3.837 7 3.301
[0073] The comparison results of the static adsorption curves of H-MFI-Zn molecular sieves for ethane gas in Examples 1, 2, 3, and 4 are as follows: Figure 6 shown.
[0074] <Example 5>
[0075] According to the results of sample gas adsorption, the H-MFI-Zn / 20 sample with a relatively large proportion of transition metal atomic mass and no obvious decrease in gas adsorption effect was selected for subsequent isomorphous substitution experiments.
[0076] 0.3713g of deionized water was added to 6.8877g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6g of TEOS (mass percentage of about 98%) and 0.3129g of zinc acetate dihydrate (mass percentage of about 98%) were added in sequence, and the initial gel solution was obtained after aging at room temperature for 12 hours. The initial solution was added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and statically crystallized for 3 hours at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction was completed, the reactor was cooled, the reaction solution was taken out, centrifuged, washed, dried, and calcined to obtain the pre-occupied Zn atom-doped MFI molecular sieve. The obtained white solid powder, 6.8877g TPAOH aqueous solution (TPAOH mass percentage = 25%) and 0.1003g SnO2 compound were stirred for 0.5h, and after being evenly mixed, they were added into a stainless steel crystallization kettle with a polytetrafluoroethylene liner and sealed, and hydrothermal crystallization was continued at a reaction temperature of 200°C and autogenous pressure for 4h. After the hydrothermal reaction, a molecular sieve solid-liquid mixture is obtained. The solid-liquid mixture after the reaction is taken out from the lining of the crystallization kettle, centrifuged at 9000R / min for 6 minutes, washed with deionized water, and repeated three times to obtain a solid product, which is dried in an oven at 110°C to remove water overnight. The sample is then ground into powder in an agate mortar and heated to 580°C at a rate of 2°C / min in a muffle furnace, maintained at 580°C for 6 hours to fully volatilize the water and organic matter therein, and then cooled to 80°C to obtain H-MFI-Zn / 20-Sn (the naming rule for all homemade molecular sieves is: H-MFI-Zn / 20-Sn, where H is the balanced cation type, MFI is the molecular sieve configuration, Zn is the pre-occupied atom type, 20 is the molar ratio of silicon to pre-occupied atoms, and Sn is the isomorphous substitution element, the same below). The calcined samples were taken out and placed in a drying dish for storage. The obtained products were analyzed by XRD for product crystal phase. The interplanar spacing of characteristic peaks in H-MFI-Zn / 20-Sn is shown in Table 5. The schematic diagram of XRD is shown in Figure 7 , indicating that the synthesized molecular sieve has the MFI molecular sieve configuration recognized by IZA, and ICP element analysis was performed on it. The analysis results showed that the Si / Sn molar ratio of the zeolite molecular sieve was 237, of which the mass percentage of Sn element in the molecular sieve sample was 0.06%.
[0077] The above-mentioned H-MFI-Zn / 20-Sn was used to adsorb ethane or ethylene gas. The adsorption test conditions were repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 20-Sn is shown in Table 12.
[0078] The ethane and ethylene gas adsorption penetration curve of the sample was measured on the 8860 series gas chromatograph of Agilent. The composition of the adsorbed mixed gas is ethane: ethylene: nitrogen = 1:1:8 (volume ratio), the total flow rate of the mixed gas is 15ml / min, and the mass of the molecular sieve adsorbent is 2.1g. First, the peak of each pure gas component molecule in the detector is tested. After the peak area error of each component is within 1%, the valve is switched to pass the raw mixed gas into the reaction tube, and the outlet of the reaction tube is connected to the automatic injection port of the gas chromatography. The gas chromatography is started for testing. After obtaining the test results, the gas phase penetration curve of the ethane-ethylene adsorption system is obtained by comparing the peak area of each component of the mixer at the outlet of the reaction tube with that of each component of the pure gas. The schematic diagram is shown in the figure. Figure 8 As shown, the dynamic adsorption capacity and selectivity of H-MFI-Zn / 20-Sn molecular sieve adsorbent for ethane and ethylene gas at a partial pressure of 0.1 bar are shown in Table 14.
[0079] Table 5 Characteristic interplanar spacing of H-MFI-Zn / 20-Sn
[0080]
[0081]
[0082] Example 6
[0083] 0.3713g of deionized water was added to 6.8877g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6g of TEOS (mass percentage of about 98%) and 0.3129g of zinc acetate dihydrate (mass percentage of about 98%) were added in sequence, and the initial gel solution was obtained after aging at room temperature for 12 hours. The initial solution was added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and statically crystallized for 3 hours at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction was completed, the reactor was cooled, the reaction solution was taken out, centrifuged, washed, dried, and calcined to obtain the MFI molecular sieve doped with pre-occupied atoms. The obtained white solid powder, 6.8877g TPAOH aqueous solution (TPAOH mass percentage = 25%) and 0.0904g TiO2 compound were stirred for 0.5h, mixed evenly, added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and continued hydrothermal crystallization for 4h at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction, a molecular sieve solid-liquid mixture was obtained. The solid-liquid mixture after the reaction was taken out from the crystallization kettle liner, centrifuged at 9000R / min for 6min, washed with deionized water, and repeated three times to obtain a solid product, which was dried and dehydrated in a 110°C oven overnight, and then the sample was ground into powder in an agate mortar, heated to 580°C at a rate of 2°C / min in a muffle furnace, maintained at 580°C for 6h, and the moisture and organic matter therein were fully volatilized, and then cooled to 80°C to obtain H-MFI-Zn / 20-Ti. The calcined sample was taken out and placed in a drying dish for storage. The product was analyzed by XRD. The interplanar spacing of the characteristic peaks in H-MFI-Zn / 20-Ti is shown in Table 6. The schematic diagram of XRD is shown in Fig. 9 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0084] The above-mentioned H-MFI-Zn / 20-Ti is used to adsorb ethane or ethylene gas. The adsorption test conditions are repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 20-Ti is shown in Table 12.
[0085] The ethane and ethylene gas adsorption penetration curve of the sample was measured on the 8860 series gas chromatograph of Agilent. The composition of the adsorbed mixed gas is ethane: ethylene: nitrogen = 1: 1: 8 (volume ratio), the total flow rate of the mixed gas is 15 ml / min, and the mass of the molecular sieve adsorbent is 2.1 g. First, the peak of each pure gas component molecule in the detector is tested. After the peak area error of each component is within 1%, the valve is switched to pass the raw mixed gas into the reaction tube. The outlet of the reaction tube is connected to the automatic injection port of the gas chromatography, and the gas chromatography is started for testing. After obtaining the test results, the gas phase penetration curve of the ethane-ethylene adsorption system is obtained by comparing the peak area of each component of the mixer at the outlet of the reaction tube with that of each component of the pure gas. The schematic diagram is shown in the figure. Fig.10 As shown, the dynamic adsorption capacity and selectivity of H-MFI-Zn / 20-Ti molecular sieve adsorbent for ethane and ethylene gas at a partial pressure of 0.1 bar are shown in Table 14.
[0086] Table 6 Characteristic interplanar spacing of H-MFI-Zn / 20-Ti
[0087] Interplanar spacing (d) 1 11.113 2 9.993 3 6.681 4 4.352 5 4.071 6 3.843 7 3.741
[0088] <Example 7>
[0089] 0.3713g of deionized water was added to 6.8877g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6g of TEOS (mass percentage of about 98%) and 0.3129g of zinc acetate dihydrate (mass percentage of about 98%) were added in sequence, and the initial gel solution was obtained after aging at room temperature for 12 hours. The initial solution was added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and statically crystallized for 3 hours at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction was completed, the reactor was cooled, the reaction solution was taken out, centrifuged, washed, dried, and calcined to obtain the pre-occupied Zn atom-doped MFI molecular sieve. The obtained white solid powder, 6.8877g TPAOH aqueous solution (TPAOH mass percentage = 25%) and 0.3494g Mn (CH3COO) 2 · 4H2O were stirred for 0.5h, and after being mixed evenly, they were added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and hydrothermal crystallization was continued for 4h at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction, a molecular sieve solid-liquid mixture was obtained. The solid-liquid mixture obtained by the reaction was taken out from the lining of the crystallization kettle, centrifuged at 9000R / min for 6min, and washed with deionized water, and repeated three times to obtain a solid product, which was dried and dehydrated in an oven at 110°C overnight, and then the sample was ground into powder in an agate mortar, heated to 580°C at a rate of 2°C / min in a muffle furnace, maintained at 580°C for 6h, and the water and organic matter therein were fully volatilized, and then cooled to 80°C to obtain H-MFI-Zn / 20-Mn. The calcined samples were taken out and placed in a drying dish for storage. The obtained products were analyzed by XRD for product crystal phase. The interplanar spacing of characteristic peaks in H-MFI-Zn / 20-Mn is shown in Table 7. The schematic diagram of XRD is shown in Fig.11 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0090] The above-mentioned H-MFI-Zn / 20-Mn was used to adsorb ethane or ethylene gas. The adsorption test conditions were repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 20-Mn is shown in Table 12.
[0091] The ethane and ethylene gas adsorption penetration curve of the sample was measured on the 8860 series gas chromatograph of Agilent. The composition of the adsorbed mixed gas is ethane: ethylene: nitrogen = 1: 1: 8 (volume ratio), the total flow rate of the mixed gas is 15 ml / min, and the mass of the molecular sieve adsorbent is 2.1 g. First, the peak of each pure gas component molecule in the detector is tested. After the peak area error of each component is within 1%, the valve is switched to pass the raw mixed gas into the reaction tube. The outlet of the reaction tube is connected to the automatic injection port of the gas chromatography, and the gas chromatography is started for testing. After obtaining the test results, the gas phase penetration curve of ethane-ethylene is obtained by comparing the peak area of each component of the mixer at the outlet of the reaction tube with that of each component of the pure gas. The schematic diagram is shown in the figure. Fig.12 As shown, the dynamic adsorption capacity and selectivity of H-MFI-Zn / 20-Mn molecular sieve adsorbent for ethane and ethylene gas at a partial pressure of 0.1 bar are shown in Table 14.
[0092] Table 7 Characteristic interplanar spacing of H-MFI-Zn / 20-Mn
[0093] Interplanar spacing (d) 1 11.110 2 9.973 3 6.353 4 4.360 5 4.000 6 3.842 7 3.753
[0094] <Example 8>
[0095] 0.3713g of deionized water was added to 6.8877g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6g of TEOS (mass percentage of about 98%) and 0.3129g of zinc acetate dihydrate (mass percentage of about 98%) were added in sequence, and the initial gel solution was obtained after aging at room temperature for 12 hours. The initial solution was added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and statically crystallized for 3 hours at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction was completed, the reactor was cooled, the reaction solution was taken out, centrifuged, washed, dried, and calcined to obtain the pre-occupied Zn atom-doped MFI molecular sieve. The obtained white solid powder, 6.8877g TPAOH aqueous solution (TPAOH mass percentage = 25%) and 0.2846g Cu(CH3COO)2·H2O were stirred for 0.5h, and after being mixed evenly, they were added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and hydrothermal crystallization was continued for 4h at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction, a molecular sieve solid-liquid mixture was obtained. The solid-liquid mixture obtained by the reaction was taken out from the lining of the crystallization kettle, centrifuged at 9000R / min for 6min, and washed with deionized water, and repeated three times to obtain a solid product, which was dried and dehydrated in an oven at 110°C overnight, and then the sample was ground into powder in an agate mortar, heated to 580°C at a rate of 2°C / min in a muffle furnace, maintained at 580°C for 6h, and the water and organic matter therein were fully volatilized, and then cooled to 80°C to obtain H-MFI-Zn / 20-Cu. The calcined sample was taken out and placed in a drying dish for storage. The product was analyzed by XRD. The interplanar spacing of the characteristic peaks in H-MFI-Zn / 20-Cu is shown in Table 8. The schematic diagram of XRD is shown in Fig.13 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0096] The above H-MFI-Zn / 20-Cu was used to adsorb ethane or ethylene gas. The adsorption test conditions were repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 20-Cu is shown in Table 12.
[0097] The ethane and ethylene gas adsorption penetration curve of the sample was measured on the 8860 series gas chromatograph of Agilent. The composition of the adsorbed mixed gas is ethane: ethylene: nitrogen = 1: 1: 8 (volume ratio), the total flow rate of the mixed gas is 15 ml / min, and the mass of the molecular sieve adsorbent is 2.1 g. First, the peak of each pure gas component molecule in the detector is tested. After the peak area error of each component is within 1%, the valve is switched to pass the raw mixed gas into the reaction tube. The outlet of the reaction tube is connected to the automatic injection port of the gas chromatography, and the gas chromatography is started for testing. After obtaining the test results, the gas phase penetration curve of ethane-ethylene is obtained by comparing the peak area of each component of the mixer at the outlet of the reaction tube with that of each component of the pure gas. The schematic diagram is shown in the figure. Fig.14 As shown, the dynamic adsorption capacity and selectivity of H-MFI-Zn / 20-Cu molecular sieve adsorbent for ethane and ethylene gases at a partial pressure of 0.1 bar are shown in Table 14.
[0098] Table 8 Characteristic interplanar spacing of H-MFI-Zn / 20-Cu
[0099] Interplanar spacing (d) 1 11.112 2 9.993 3 6.682 4 4.351 5 4.033 6 3.852 7 3.712
[0100] <Example 9>
[0101] 0.3713g of deionized water was added to 6.8877g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6g of TEOS (mass percentage of about 98%) and 0.3129g of zinc acetate dihydrate (mass percentage of about 98%) were added in sequence, and the initial gel solution was obtained after aging at room temperature for 12 hours. The initial solution was added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and statically crystallized for 3 hours at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction was completed, the reactor was cooled, the reaction solution was taken out, centrifuged, washed, dried, and calcined to obtain the pre-occupied Zn atom-doped MFI molecular sieve. The obtained white solid powder, 6.8877g TPAOH aqueous solution (TPAOH mass percentage = 25%) and 0.3583g Ni (CH3COO) 2 · 4H2O were stirred for 0.5h, and after being mixed evenly, they were added to a stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and sealed, and hydrothermal crystallization was continued for 4h at a reaction temperature of 200°C and autogenous pressure. After the hydrothermal reaction, a molecular sieve solid-liquid mixture was obtained. The solid-liquid mixture obtained by the reaction was taken out from the lining of the crystallization kettle, centrifuged at 9000R / min for 6min, and washed with deionized water, and repeated three times to obtain a solid product, which was dried and dehydrated in an oven at 110°C overnight, and then the sample was ground into powder in an agate mortar, heated to 580°C at a rate of 2°C / min in a muffle furnace, maintained at 580°C for 6h, and the water and organic matter therein were fully volatilized, and then cooled to 80°C to obtain H-MFI-Zn / 20-Ni. The calcined sample was taken out and placed in a drying dish for storage. The product was analyzed by XRD. The interplanar spacing of the characteristic peaks in H-MFI-Zn / 20-Ni is shown in Table 9. The schematic diagram of XRD is shown in Fig.15 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0102] The above H-MFI-Zn / 20-N was used to adsorb ethane or ethylene gas, and the adsorption test conditions were repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Zn / 20-Ni is shown in Table 12.
[0103] The ethane and ethylene gas adsorption penetration curve of the sample was measured on the 8860 series gas chromatograph of Agilent. The composition of the adsorbed mixed gas is ethane: ethylene: nitrogen = 1: 1: 8 (volume ratio), the total flow rate of the mixed gas is 15 ml / min, and the mass of the molecular sieve adsorbent is 2.1 g. First, the peak of each pure gas component molecule in the detector is tested. After the peak area error of each component is within 1%, the valve is switched to pass the raw mixed gas into the reaction tube. The outlet of the reaction tube is connected to the automatic injection port of the gas chromatography, and the gas chromatography is started for testing. After obtaining the test results, the gas phase penetration curve of ethane-ethylene is obtained by comparing the peak area of each component of the mixer at the outlet of the reaction tube with that of each component of the pure gas. The schematic diagram is shown in the figure. Fig.16 As shown, the dynamic adsorption capacity and selectivity of H-MFI-Zn / 20-Ni molecular sieve adsorbent for ethane and ethylene gas at a partial pressure of 0.1 bar are shown in Table 14.
[0104] Table 9 Characteristic interplanar spacing of H-MFI-Zn / 20-Ni
[0105] Interplanar spacing (d) 1 11.038 2 9.993 3 6.660 4 4.345 5 4.003 6 3.842 7 3.736
[0106] <Comparative Example 1>
[0107] 0.3713 g of deionized water was added to 6.8877 g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6 g of TEOS (mass percentage about 98%) and 0.1003 g of SnO2 were added in sequence and aged at room temperature for 12 hours to obtain an initial gel solution. The initial gel solution was added to a sealed stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and hydrothermally crystallized at a reaction temperature of 200° C. and autogenous pressure for 3 hours. After the hydrothermal reaction, a molecular sieve solid-liquid mixture is obtained. The solid-liquid mixture obtained by the reaction is taken out from the lining of the crystallization kettle, centrifuged at 9000R / min for 6 minutes, and washed with deionized water. The process is repeated three times to obtain a solid product, which is dried in an oven at 110°C to remove water overnight. The sample is then ground into powder in an agate mortar, heated to 580°C at a rate of 2°C / min in a muffle furnace, maintained at 580°C for 6 hours, and the water and organic matter therein are fully volatilized. The mixture is then cooled to 80°C to obtain H-MFI-Sn / 20. The calcined sample is taken out and placed in a drying dish for storage. The product is analyzed for crystal phase by XRD. The interplanar spacing of the characteristic peaks in H-MFI-Sn / 20 is shown in Table 10, and the schematic diagram of XRD is shown in Fig.17 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0108] The above H-MFI-Sn / 20 was used to adsorb ethane or ethylene gas. The adsorption test conditions were repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Sn / 20 is shown in Table 12.
[0109] The ethane and ethylene gas adsorption penetration curve of the sample was measured on the 8860 series gas chromatograph of Agilent. The composition of the adsorbed mixed gas is ethane: ethylene: nitrogen = 1: 1: 8 (volume ratio), the total flow rate of the mixed gas is 15 ml / min, and the mass of the molecular sieve adsorbent is 2.1 g. First, the peak of each pure gas component molecule in the detector is tested. After the peak area error of each component is within 1%, the valve is switched to pass the raw mixed gas into the reaction tube. The outlet of the reaction tube is connected to the automatic injection port of the gas chromatography, and the gas chromatography is started for testing. After obtaining the test results, the gas phase penetration curve of ethane-ethylene is obtained by comparing the peak area of each component of the mixer at the outlet of the reaction tube with that of each component of the pure gas. The schematic diagram is shown in the figure. Fig.18 As shown, the dynamic adsorption capacity and selectivity of H-MFI-Sn / 20 molecular sieve adsorbent for ethane and ethylene gas at a partial pressure of 0.1 bar are shown in Table 14.
[0110] Table 10 Characteristic interplanar spacing of H-MFI-Sn / 20
[0111] Interplanar spacing (d) 1 11.065 2 9.940 3 6.679 4 4.353 5 3.994 6 3.835 7 3.748
[0112] <Comparative Example 2>
[0113] 0.3713 g of deionized water was added to 6.8877 g of TPAOH aqueous solution (TPAOH mass percentage = 25%), and then 6 g of TEOS (mass percentage about 98%) and 0.3494 g of Mn(CH3COO)2·4H2O were added in sequence and aged at room temperature for 12 h to obtain an initial gel solution. The initial gel solution was added to a sealed stainless steel crystallization kettle equipped with a polytetrafluoroethylene liner and hydrothermally crystallized at a reaction temperature of 200°C and autogenous pressure for 3 h. After the hydrothermal reaction, a molecular sieve solid-liquid mixture is obtained. The solid-liquid mixture obtained by the reaction is taken out from the lining of the crystallization kettle, centrifuged at 9000R / min for 6 minutes, and washed with deionized water. The process is repeated three times to obtain a solid product, which is dried in an oven at 110°C to remove water overnight. The sample is then ground into powder in an agate mortar, heated to 580°C at a rate of 2°C / min in a muffle furnace, maintained at 580°C for 6 hours, and the water and organic matter therein are fully volatilized. The mixture is then cooled to 80°C to obtain H-MFI-Mn / 20. The calcined sample is taken out and placed in a drying dish for storage. The product is analyzed for crystal phase by XRD. The interplanar spacing of the characteristic peaks in H-MFI-Mn / 20 is shown in Table 11, and the schematic diagram of XRD is shown in Fig.19 , indicating that the synthesized zeolite has the MFI zeolite configuration recognized by IZA.
[0114] The above H-MFI-Mn / 20 was used to adsorb ethane or ethylene gas. The adsorption test conditions were repeated in Example 1. The static adsorption amount of ethane and ethylene gas by H-MFI-Mn / 20 is shown in Table 12.
[0115] The ethane and ethylene gas adsorption penetration curve of the sample was measured on the 8860 series gas chromatograph of Agilent. The composition of the adsorbed mixed gas is ethane: ethylene: nitrogen = 1: 1: 8 (volume ratio), the total flow rate of the mixed gas is 15 ml / min, and the mass of the molecular sieve adsorbent is 2.1 g. First, the peak of each pure gas component molecule in the detector is tested. After the peak area error of each component is within 1%, the valve is switched to pass the raw mixed gas into the reaction tube. The outlet of the reaction tube is connected to the automatic injection port of the gas chromatography, and the gas chromatography is started for testing. After obtaining the test results, the gas phase penetration curve of ethane-ethylene is obtained by comparing the peak area of each component of the mixer at the outlet of the reaction tube with that of each component of the pure gas. The schematic diagram is shown in the figure. Fig. 20 As shown, the dynamic adsorption capacity and selectivity of H-MFI-Mn / 20 molecular sieve adsorbent for ethane and ethylene gas at a partial pressure of 0.1 bar are shown in Table 14.
[0116] Table 11 Characteristic interplanar spacing of H-MFI-Mn / 20
[0117] Interplanar spacing (d) 1 11.168 2 10.025 3 6.729 4 4.369 5 4.007 6 3.847 7 3.759
[0118] <Comparative Example 3>
[0119] Take a certain amount of commercial H-type MFI molecular sieves with different silicon-aluminum ratios (the naming rule of commercial molecular sieves is H-MFI / A, where A is the molar ratio of silicon and aluminum atoms in the molecular sieve, and commercial molecular sieves are all silicon-aluminum molecular sieves) and calcine them in air to ensure the removal of impurities: heat to 580℃ at a rate of 2℃ / min, maintain at 580℃ for 6h, and then cool to 100℃. Take out the dried sample and store it in a drying dish.
[0120] The above commercial molecular sieves were used to adsorb ethane or ethylene gas. The adsorption test conditions were repeated in Example 1. The static adsorption capacity of the commercial molecular sieves for ethane and ethylene gas is shown in Table 13.
[0121] <Comparative Example 4>
[0122] By comparing the adsorption performance, two commercial H-type MFI molecular sieves (Si / Al=50, Mizusawa Industrial Chemicals) were taken and calcined in air to ensure the removal of impurities: heated to 580°C at a rate of 2°C / min, maintained at 580°C for 6 hours, and then cooled to 100°C. The dried samples were taken out and stored in a desiccating dish.
[0123] At the same time, the above samples were used for ethane-ethylene adsorption separation. The ethane-ethylene gas adsorption penetration curve of the sample was measured on a 8860 series gas chromatograph from Agilent. The composition of the adsorbed mixed gas is ethane: ethylene: nitrogen = 1:1:8 (volume ratio), the total flow rate of the mixed gas is 15 ml / min, the mass of the molecular sieve adsorbent is 2.1 g, and the peak conditions of each pure gas component molecule in the detector are tested first. After the peak area error of each component is within 1%, the valve is switched to pass the raw mixed gas into the reaction tube, and the outlet of the reaction tube is connected to the automatic injection port of the gas chromatography. The gas chromatography is started for testing. After the test results are obtained, the gas phase penetration curve of the ethane-ethylene adsorption system is obtained by comparing the peak areas of each component of the mixer at the outlet of the reaction tube with those of the pure gas. The schematic diagram is shown in the figure. Fig.21 As shown, the dynamic adsorption capacity of commercial molecular sieve adsorbents and isomorphously substituted molecular sieve products for ethane and ethylene gases at a partial pressure of 0.1 bar, and the adsorption selectivity comparison is shown in Table 14.
[0124] Table 12298K static adsorption of ethane and ethylene by different molecular sieves in the examples
[0125]
[0126] Table 13298K static adsorption of ethane and ethylene gas by different molecular sieves and one-step method in comparative examples
[0127]
[0128] Table 14 Dynamic adsorption capacity and adsorption selectivity of H-MFI-Zn / 20+Sn, H-MFI-Zn / 20+Ti, H-MFI-Zn / 20+Mn, H-MFI-Sn / 20 and H-MFI / 50 for ethane and ethylene at 298K
[0129]
[0130] The contents described in this specification are merely an enumeration of implementation forms of the inventive concept, and the protection scope of the present invention should not be regarded as being limited to the specific forms described in the embodiments.
Claims
1. A transition metal atom pre-occupied MFI molecular sieve with secondary hydrothermal isomorphous substitution, Features The molecular sieve has the MFI molecular sieve configuration recognized by the International Molecular Sieve Association (IZA). The preparation method of the molecular sieve adopts the method that zinc atoms occupy specific skeleton positions in the preliminary hydrothermal synthesis, wash and roast after the crystal is stable, and then mix with W isomorphous substitution raw materials, alkaline template agent and water, and perform secondary hydrothermal synthesis to achieve isomorphous substitution. The chemical composition molar ratio of the obtained molecular sieve product is aYO 2 :bZnO:cH 2 O: dWOx, wherein 10≤a≤40, 0.025≤b≤1, 0<c≤11, 0.0125≤d≤1, Y is a tetravalent element, including one or more of Si, Ge, and Sn, W is an isomorphous substitution element after crystallization stabilization, including Ni, Mn, Cu, Ti, or Sn, and WOx is SnO 2 、TiO 2 , MnO, CuO or NiO; and when measured by X-ray diffraction, the MFI molecular sieve has characteristic peaks within at least the following four crystal plane spacings (d), the first crystal plane spacing d=11.0±0.3, the second crystal plane spacing d=9.9±0.2, the third crystal plane spacing d=4.3±0.2, and the fourth crystal plane spacing d=3.8±0.
2.
2. A transition metal atom pre-occupied and secondary hydrothermal isomorphously substituted molecular sieve as claimed in claim 1, Features The elemental composition contains more tetravalent element Si, less divalent transition metal element zinc and isomorphous substitution element W. Determined by inductively coupled plasma spectroscopy, 10≤a≤20, 0.05≤b≤0.4, 0<c≤2.5, 0.05≤d≤0.
1.
3. A molecular sieve with transition metal atom pre-occupancy and secondary hydrothermal isomorphous substitution as claimed in claim 1, Features Y is Si element.
4. A method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to any one of claims 1 to 3, Features The method is carried out according to the following steps: a precursor gel solution is formed by mixing aqueous solutions of at least a basic template, zinc acetate and a compound raw material of a tetravalent element Y, and a solid-liquid mixture of a molecular sieve doped with a metal zinc skeleton is obtained after a hydrothermal synthesis reaction; the molecular sieve solid-liquid mixture is then centrifuged, washed, and dried, and then placed in an air atmosphere for high-temperature calcination, and then the obtained solid powder, the basic template, the W isomorphous substitution raw material and water are mixed and stirred uniformly, and a secondary hydrothermal synthesis is continued, and isomorphous substitution is achieved by concentration difference substitution of the zinc element in the molecular sieve skeleton by a high concentration of W element to obtain a solid-liquid mixture of a new metal atom isomorphous substitution molecular sieve, and then the molecular sieve solid powder according to claims 1 to 3 is obtained by centrifugation, washing, drying and roasting.
5. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 4, Features The specific steps include: (a) Add alkaline template and deionized water into the reaction kettle in sequence, heat and stir to fully dissolve and mix, and then add (10-40)YO 2 : The zinc acetate and the compound raw material containing the tetravalent element Y in the above molecular sieve composition are added in a molar ratio of 1:10 ... (b) centrifuging, washing, drying, grinding, and then calcining and activating the molecular sieve solid-liquid mixture obtained in step (a) in an air atmosphere to remove organic matter in the molecular sieve solid-liquid mixture to obtain a solid powder; (c) the solid powder obtained in step (b), the alkaline template, the W isomorphous substitution raw material and water are uniformly stirred, and secondary hydrothermal crystallization is continued to achieve isomorphous substitution by the concentration difference substitution of the zinc element in the molecular sieve framework by the high concentration of W element, and then the solid-liquid mixture of the molecular sieve is obtained by centrifugation, washing, drying and roasting; the alkaline template is tetrapropylammonium hydroxide.
6. A method for preparing a transition metal atom pre-occupied isomorphously substituted molecular sieve as claimed in claim 5, Features In step (a), the mass ratio of deionized water to tetrapropylammonium hydroxide is 2-6:1; the mass of tetrapropylammonium hydroxide is 25-30% of the mass of the compound raw material containing the tetravalent element Y.
7. A method for preparing a transition metal atom pre-occupied isomorphously substituted molecular sieve as claimed in claim 6, Features In step (a), the mass ratio of deionized water to tetrapropylammonium hydroxide is 3-3.5:1; the mass of tetrapropylammonium hydroxide is 25% of the mass of the compound raw material containing the tetravalent element Y.
8. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 5, Features In step (a), the aging time is selected to be 12-24 hours; the aging temperature is selected to be room temperature; the reaction temperature of the hydrothermal synthesis is 180-220° C.; the reaction time of the hydrothermal synthesis is the molecular sieve crystal stability time, which is selected to be 2.8-3.2 hours.
9. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 8, Features In step (a), the aging time is selected to be 12-16 hours; the reaction temperature of the hydrothermal synthesis is 200° C.; and the reaction time of the hydrothermal synthesis is 3 hours.
10. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 5, Features In step (b), the drying process temperature is selected to be 60-150°C, and the drying time is selected to be 2-24h. The dried molecular sieve solid-liquid mixture needs to be heated and calcined to remove the internal template agent so that it has adsorption and catalytic properties. The calcination temperature is selected to be 400-700°C, and the constant temperature calcination time is selected to be 2-12h.
11. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 10, Features In step (b), the drying process temperature is selected to be 80-120° C., the calcination temperature is selected to be 500-600° C., and the constant temperature calcination time is selected to be 3-8 hours.
12. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 11, Features In step (b), the constant temperature calcination time is selected to be 4-7h.
13. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 5, Features In step (c), the stirring time is selected to be 0.1-1h, the stirring temperature is selected to be 10-50°C, the crystallization temperature in step (c) is the same as the hydrothermal synthesis temperature in step (a), the crystallization time is selected to be 1-8h, and the calcination temperature and time in step (c) are the same as those in step (b).
14. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 13, Features In step (c), the stirring time is selected to be 0.5-1 h, the stirring temperature is selected to be 20-30° C., and the crystallization time in step (c) is selected to be 2-6 h.
15. The method for preparing a transition metal atom pre-occupied secondary hydrothermal isomorphous substitution molecular sieve according to claim 14, Features In step (c), the crystallization time is selected to be 4-5h.
16. Use of the transition metal atom pre-occupancy-secondary hydrothermal isomorphous substitution molecular sieve as claimed in claim 1, Features The molecular sieve is used for selective adsorption separation of ethane-ethylene mixed gas, and preferentially adsorbs a large amount of ethane gas in the mixed gas.
Citation Information
Patent Citations
Method for separating ethane and ethylene in mixed gas
CN103058810A
Heteroatom zeolite adsorbent and preparation method thereof
CN104549141A
Application of flexible material TUT-3 serving as adsorbent to separating ethane from ethylene
CN105709693A
Adsorption and separation agent for separation of ethylene and ethane as well as preparation method and application thereof
CN108187607A
An MFI-type molecular sieve catalyst with a tungsten framework, its preparation method, and its catalytic application.
CN109513458B
Cited By
Method for improving adsorption separation performance of molecular sieve
CN120662263A