A low-cost simplified process for preparing high-purity cesium salt and high-purity rubidium salt
By using high-purity CO2 for carbonization in the preparation process of high-purity cesium salts and rubidium salts, the process flow is simplified, the problems of high extraction agent cost and complex equipment in the existing technology are solved, and a low-cost, high-efficiency high-efficiency process is achieved. Production of pure cesium salts and rubidium salts.
Patent Information
- Application Number
- CN202310398554.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-14
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-04-14
AI Technical Summary
The extraction agent t-BAMBP used in the existing high-purity cesium salt and rubidium salt preparation processes is high in cost, and the process equipment is complex and expensive, resulting in excessive production and equipment costs.
High-purity CO2 is directly introduced into the cesium extraction residual liquid for carbonization treatment to generate rubidium carbonized liquid. The use of extraction agents such as t-BAMBP is omitted, and the process flow is simplified. After potassium and aluminum removal, cesium extraction and back-extraction are performed. , control pH value to achieve rubidium carbonization, reducing process and equipment requirements.
Significantly shorten the process cycle and equipment costs, reduce reagent costs, improve production efficiency, reduce pollution and environmental protection equipment investment, and product purity and yield meet or exceed the original process standards.
Smart Images

Figure CN116477645B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of alkali metal element extraction, and specifically relates to a low-cost simplified process for preparing two products, a high-purity cesium salt and a high-purity rubidium salt. Background Art
[0002] Due to its unique properties, rubidium and cesium have important uses in many fields. Not only do they have many traditional application fields, but also some new application fields have emerged. Especially in some high-tech fields, rubidium and cesium have shown an increasingly important role. Rubidium and cesium have made great progress in traditional application fields such as electronic devices, catalysts, special glass, biochemistry and medicine in the past 10 years; and in new application fields such as magnetohydrodynamic power generation, thermal ion conversion power generation, ion propulsion engines, laser energy conversion power devices, and cesium ion cloud communications, rubidium and cesium have also shown strong vitality. At present, the main raw materials for the industrial production of rubidium and cesium salts in the world are cesium garnet and lithium mica. Rubidium and cesium are active in nature, easily lose their outer electrons, and exist in the form of soluble salts in solution. Rubidium and cesium are abundant in nature, but the content is low, and they often coexist with other alkali metals such as lithium, sodium, and potassium. In the prior art, the extraction methods of rubidium and cesium include precipitation, ion exchange, and extraction.
[0003] Chinese application CN115725855A discloses a method for preparing high-purity cesium salt and high-purity rubidium salt, wherein tartaric acid is added to a rubidium cesium alum solution containing potassium, potassium and tartaric acid are used to generate potassium tartrate, and cooling and recrystallization are performed so that rubidium cesium alum is precipitated in the form of crystals to obtain rubidium cesium alum crystals without potassium. The rubidium cesium alum crystals are dissolved in water again, aluminum is precipitated by an aluminum removal agent, and a purified cesium rubidium salt solution is obtained, and cesium extraction is performed on the purified cesium rubidium salt solution to obtain a cesium extraction organic phase and cesium extraction residual water, and then the cesium extraction organic phase is stripped with ammonium salt or acid as a stripping agent to obtain a cesium stripping solution. After adding alkali to the cesium extraction residual water to adjust the pH, an extractant is added to obtain a rubidium extraction organic phase, and then a stripping agent is used to strip the rubidium extraction organic phase to obtain a rubidium stripping solution. Finally, the cesium stripping solution and the rubidium stripping solution are respectively finely filtered, and then evaporated, concentrated, dried, calcined, re-dissolved and dried again to obtain high-purity cesium salt and high-purity rubidium salt. The extractant used for cesium extraction and rubidium extraction is a mixture of t-BAMBP, diethylbenzene and kerosene. For another example, CN104016384A discloses a method for producing high-purity cesium carbonate and high-purity rubidium carbonate, which comprises using t-BAMBP as an extractant, sulfonated kerosene and diethylbenzene as diluents to separate cesium, using high-purity oxalic acid to prepare a stripping acid to extract cesium from the cesium organic extraction phase to obtain cesium oxalate; then using t-BAMBP as an extractant, sulfonated kerosene and xylene as diluents to extract rubidium from the cesium raffinate, using high-purity oxalic acid to prepare a stripping acid to extract rubidium from the rubidium organic extraction phase to obtain rubidium oxalate; crystallizing through a recrystallization device to obtain cesium oxalate and rubidium oxalate crystals, respectively, and then calcining to obtain high-purity cesium carbonate and high-purity rubidium carbonate.
[0004] In all the above processes, the cesium raffinate needs to be extracted with an organic phase containing t-BAMBP to obtain an organic phase for extracting rubidium, and the organic phase is stripped with acid, and then finely filtered and recrystallized to obtain a high-purity rubidium salt. The organic phase containing t-BAMBP is used twice to extract cesium and rubidium successively, and the consumption of the extractant is large. However, t-BAMBP is expensive, about 300,000 yuan / t, resulting in high process costs. In addition, the rubidium extraction process of the cesium raffinate needs to be equipped with a special pH-adjusting stirring tank and a centrifugal extractor of about 12 stages, and the equipment cost is also high. Based on the above reasons, it is necessary to improve the existing preparation process of high-purity cesium salt and rubidium salt. Summary of the invention
[0005] 1. Technical issues to be resolved
[0006] In view of the above-mentioned shortcomings and deficiencies of the prior art, the present invention provides a low-cost simplified process for preparing two products, high-purity cesium salt and high-purity rubidium salt. By simplifying the existing process for preparing high-purity cesium salt and high-purity rubidium salt, the purpose of greatly reducing reagent costs and equipment costs is achieved, while shortening the process and improving production efficiency.
[0007] (II) Technical solution
[0008] A low-cost simplified process for preparing two products, high-purity cesium salt and high-purity rubidium salt, comprising:
[0009] S1, removing potassium and aluminum from a mixed solution containing rubidium, cesium and potassium to obtain a purified rubidium-cesium salt solution;
[0010] S2, extracting cesium from the purified rubidium-cesium salt solution to obtain a cesium-extracted organic phase and a cesium-extracted residual solution; washing the cesium-extracted organic phase; stripping the washed cesium-extracted organic phase with a stripping agent to obtain a cesium stripping solution; finely filtering the cesium stripping solution, and sequentially evaporating, concentrating, crystallizing, drying, calcining, recrystallizing, and then drying to obtain a high-purity cesium salt;
[0011] S3, pass high-purity CO into the cesium extraction residue 2 When the pH value no longer changes (usually reaches 8-9), filter to obtain rubidium carbonization liquid and carbonate impurity salt precipitation; accurately filter the rubidium carbonization liquid, evaporate, concentrate and crystallize the filtrate, dry and calcine, recrystallize and dry again to obtain high-purity rubidium carbonate.
[0012] According to a preferred embodiment of the present invention, in S1, the mixed solution containing rubidium, cesium and potassium is obtained by dissolving a mixed alum containing rubidium, cesium and potassium in deionized water.
[0013] The mixed solution containing rubidium, cesium and potassium can be prepared from acidic mixed alum and alkaline mixed salt, and the mixed solution can be an acidic solution or an alkaline solution. Acidic mixed alum is the most ideal raw material, which can be directly treated to remove potassium and aluminum. Other raw materials need to be converted into alum by adding reagents, and then processed according to the process of the present invention. However, it should be noted that the raw materials applicable to the process of the present invention are any raw materials containing rubidium and cesium, regardless of the content of potassium and sodium, as long as they can be converted into alum by reagent reaction first, and then processed according to the process of the present invention, two products of cesium salt and rubidium salt with a purity of more than 99.9% can be obtained. For some raw materials containing cesium and rubidium potassium that are not alum, they need to be converted into alum by adding reagents first, and then recrystallized to obtain purified cesium and rubidium alum, and then operated according to the process of the present invention.
[0014] According to a preferred embodiment of the present invention, in S1, the potassium removal method comprises: adding tartaric acid to the mixed solution containing rubidium, cesium and potassium, wherein the molar ratio of tartaric acid to potassium in the mixed solution containing rubidium, cesium and potassium is 0.2-0.7, heating to a temperature of 50-95°C, reacting for 1-3 hours, standing for 12-24 hours, cooling for recrystallization, centrifuging, precipitating rubidium salt and cesium salt in the form of crystals, and retaining potassium tartrate in the solution, to obtain a potassium tartrate solution and rubidium cesium salt crystals with a potassium content of less than 0.0035%. The potassium tartrate solution is recycled.
[0015] According to a preferred embodiment of the present invention, in S1, the aluminum removal method includes: dissolving rubidium-cesium salt crystals in deionized water, adding barium hydroxide solution or calcium hydroxide solution, heating and stirring the reaction while adding, controlling the pH of the reaction end point to be 6.5-8.5, and keeping warm for 10-60 minutes after reaching the reaction end point to precipitate aluminum in the form of aluminum hydroxide; centrifuging the reaction mixture to obtain a clear liquid and a precipitated residue; and finely filtering the clear liquid to obtain a purified rubidium-cesium salt solution and a filter residue.
[0016] The barium hydroxide solution or calcium hydroxide solution is prepared by dissolving analytically pure barium hydroxide or analytically pure calcium oxide in deionized water.
[0017] According to a preferred embodiment of the present invention, in S2, before cesium extraction, the pH of the purified rubidium-cesium salt solution is adjusted to alkaline, and then finely filtered to obtain a causticized purified cesium-cesium salt solution and a filter residue; and cesium extraction is performed on the causticized purified cesium-cesium salt solution.
[0018] Preferably, before cesium extraction, calcium hydroxide or barium hydroxide solution is added to the purified rubidium-cesium salt solution, while heating and stirring the reaction, the reaction temperature is 90-97°C, the pH of the reaction endpoint is controlled to be ≥13.0, and the reaction is kept warm for 10min-60min after reaching the reaction endpoint, so that cesium is completely dissolved in the aqueous phase in the form of cesium hydroxide; after precise filtration, a causticized purified cesium-rubidium salt solution and barium slag or calcium slag are obtained; and cesium extraction is performed on the causticized purified cesium-rubidium salt solution.
[0019] According to a preferred embodiment of the present invention, in S2, the cesium extraction method is: using a mixed solvent of t-BAMBP, diethylbenzene and kerosene as an extractant, cesium extraction is performed on the causticized purified cesium rubidium salt solution to obtain a cesium extraction organic phase and a cesium extraction residual solution; using water or a dilute alkaline aqueous solution as a detergent to wash the cesium extraction organic phase to obtain a washing solution and a washed cesium extraction organic phase; after washing, using ammonium carbonate or oxalic acid as a stripping agent to strip the cesium extraction organic phase to obtain a cesium stripping solution. The cesium stripping solution is finely filtered, evaporated, concentrated, crystallized, dried, calcined, recrystallized, and then dried to obtain high-purity cesium carbonate. If sulfuric acid or nitric acid is used as a stripping agent, the product is the corresponding cesium sulfate or cesium nitrate.
[0020] According to a preferred embodiment of the present invention, after step S1, the removal rate of potassium and aluminum in the mixed solution containing rubidium, cesium and potassium reaches more than 99.9%; after step S2, the removal rate of cesium in the purified rubidium-cesium salt solution reaches more than 99.9%.
[0021] According to a preferred embodiment of the present invention, in step S3, the dissolved substance in the cesium extraction residual solution is RbOH, and the remaining impurities are mainly trace amounts of Ba, Fe, Ca, and Mg metal ions; high-purity carbon dioxide gas is introduced to cause the impure metal ions to generate carbonate precipitates, which are then precisely filtered to obtain a purified rubidium carbonized liquid; the rubidium carbonized liquid is evaporated, concentrated, and crystallized, dried, and calcined, and then redissolved in deionized water, evaporated, concentrated, and crystallized again, and dried to obtain high-purity rubidium carbonate.
[0022] In step S3, high-purity CO is introduced into the cesium extraction residue. 2 The pH is brought to 8-9, preferably pH 8.5.
[0023] Preferably, the precision filtration in the above steps is microfiltration of 0.08-0.15 μm.
[0024] (III) Beneficial effects
[0025] Compared with the prior art, the present invention omits the process of extracting rubidium from the cesium extraction residual solution using an organic phase extractant containing t-BAMBP, but directly introduces high-purity carbon dioxide into the cesium extraction residual solution for carbonization to generate rubidium carbonized liquid (a mixture of rubidium carbonate and rubidium bicarbonate). Rubidium carbonate and rubidium bicarbonate are both easily soluble in water, while trace metal impurities such as calcium, magnesium, barium and iron (generally a small amount of impurities contained in the cesium rubidium mixed alum or introduced during the aluminum removal process) in the cesium extraction residual solution are carbonized to generate carbonate insoluble particles. After precise filtration, the filtrate is a high-purity rubidium carbonized liquid, which is then evaporated, concentrated, crystallized, dried, calcined, recrystallized, and dried to obtain high-purity rubidium carbonate. By omitting the operation of extracting rubidium from the cesium extraction residual solution, the following technical effects can be achieved:
[0026] (1) Shorten process cycle, lower equipment cost, lower reagent cost, and less pollution; specifically include:
[0027] ① When the original process extracts rubidium from the cesium extractant, it is necessary to use a strong base to adjust the pH ≥ 13.0, prepare an extractant (t-BAMBP + sulfonated kerosene + diethylbenzene / dimethylbenzene) and a stripping agent, control the extraction ratio, extraction time, etc. After the improvement, it is only necessary to control the carbonization end point (pH 8-9) of the cesium extractant, reduce the rubidium extraction and stripping process and time consumption, and greatly shorten the process cycle. According to the actual operation situation, the carbonization process can be completed within 1 hour, while the original process requires at least 10 hours for the preparation of stripping agents and regeneration agents from adjusting the pH of the cesium extractant to the regeneration of the lean organic phase. Each process also needs to monitor the quality of the intermediate product and the stability of the parameters, and the product analysis and detection and adjustment of the equipment operating parameters should be carried out regularly during the period. Compared with the original process, the present invention has greatly reduced the process cycle, labor cost, reagent cost and management cost.
[0028] ② The rubidium extraction process of the original process requires a pH-adjusting stirring tank + about 15-stage centrifugal extractors + filtration equipment. The investment in the pH stirring tank and precision filtration equipment is about 10,000 yuan, and a centrifugal extractor is about 100,000 yuan. The 15-stage extraction (8-stage rubidium extraction + 4-stage back-extraction + 3-stage regeneration) requires a cost of about 1.5 million yuan, totaling 1.51 million yuan. After the improvement, only a PP carbonization tower + precision filtration equipment is required, and the equipment cost investment does not exceed 10,000 yuan. After the improvement, the equipment consumption for preparing high-purity rubidium salts is 1 / 151 of the original process, and the number of equipment and the land occupied are only 1 / 15 of the original process, and the investment cost of equipment and plant buildings is greatly reduced.
[0029] ③ The original process requires the use of t-BAMBP for rubidium extraction. t-BAMBP is a well-known rubidium-cesium special extraction agent in the industry. It is expensive, about 300,000 yuan / t. In addition, rubidium back-extraction also requires a stripping agent, a regeneration agent and pure water for reagent preparation. The improved process only requires high-purity carbon dioxide gas, and the reagent investment cost is greatly reduced.
[0030] ④ The original process will produce a large amount of rubidium extraction residue (rubidium-poor organic phase) after rubidium extraction and stripping. This part contains a small amount of t-BAMBP, diethylbenzene (or xylene) and kerosene, which need to be purified; at the same time, a small amount of organic phase will be mixed in the rubidium stripping solution, which also needs to be purified; while the improved process directly introduces high-purity carbon dioxide gas into the cesium extraction residue, without the generation of three wastes. The improved process has obvious environmental advantages and also saves the investment in environmental protection equipment.
[0031] ⑤ The original process required 3 to 4 people due to the long process, many equipments, reagent configuration and product monitoring and analysis. The simplified process only requires 1 person, which greatly reduces the labor cost. If the original process is to be automated, the cost of installing the automatic control device for the entire process is also much higher than the process provided by the present invention.
[0032] (2) Comparison of the yield of high-purity rubidium carbonate product with that of the original process: The simplified process does not require the step of adjusting the pH with a strong base, and there is no slag to carry away the rubidium. According to the actual yield calculated from the experiment, the simplified process can increase the yield by more than 2.5%.
[0033] (3) Comparison of the purity of high-purity rubidium carbonate products with that of the original process: its impurity indicators such as calcium, magnesium and lithium are better than those of the extraction process, while its potassium and sodium indicators are lower than those of the extraction process, but all of them reach the standard of more than 99.9%.
[0034] In summary, although the present invention omits the process of extracting rubidium and stripping rubidium from the cesium extraction residue using t-BAMBP and the like compared with the prior art, the purity and yield of the high-purity rubidium carbonate product are not reduced compared with the original process. It can be seen that the simplified process of the present invention can obtain two products, high-purity cesium salt and high-purity rubidium salt, and the purity and yield of the products are not lower than those of the original process. At the same time, the simplified process of the present invention has significant advantages in process cycle, equipment cost, reagent cost, environmental protection, labor, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 The present invention is a simplified process diagram for preparing two products, high-purity cesium salt and high-purity rubidium salt, at a low cost. DETAILED DESCRIPTION
[0036] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.
[0037] like Figure 1 As shown in the figure, a low-cost simplified process for preparing two products, high-purity cesium salt and high-purity rubidium salt, is provided by the present invention. The process mainly comprises introducing high-purity CO into the cesium extraction residual solution. 2 The pH is stabilized, filtered, and rubidium carbide liquid and carbonate impurity salt (carbonate of calcium, magnesium, barium, iron, etc.) are precipitated; the rubidium carbide liquid is precisely filtered, the filtrate is evaporated, concentrated, crystallized, dried, calcined, recrystallized, and dried to obtain high-purity rubidium carbonate. The present invention uses a method of directly carbonizing the cesium extraction residual liquid to replace the prior art steps of adjusting the pH to ≥ 13 with caustic soda, extracting with t-BAMBP extractant, and stripping with ammonium salt or acid as stripping agent.
[0038] Depend on Figure 1 As shown, the whole process of the low-cost simplified process for preparing two products, high-purity cesium salt and high-purity rubidium salt, includes:
[0039] Step 1: dissolving a mixed alum containing rubidium, cesium and potassium in deionized water to obtain a mixed solution containing rubidium, cesium and potassium. For some raw materials containing cesium, rubidium and potassium that are not in the form of alum, it is necessary to first convert them into alum by adding reagents, and then purify the alum by recrystallization. According to the process of the present invention, high-purity cesium salt and high-purity rubidium carbonate salt with a purity of more than 99.9% can also be obtained.
[0040] Step 2: Remove potassium from the mixed solution.
[0041] The potassium removal method comprises: adding tartaric acid to a mixed solution containing rubidium, cesium and potassium, wherein the molar ratio of tartaric acid to potassium in the mixed solution containing rubidium, cesium and potassium is 0.2-0.7, heating to a temperature of 50-95°C, reacting for 1-3 hours, standing for 12-24 hours, cooling and recrystallizing, so that rubidium and cesium salts are precipitated in the form of rubidium cesium salt crystals, potassium tartrate is retained in the solution, and a potassium tartrate solution and rubidium cesium salt crystals with a potassium content of less than 0.0035% are obtained. The potassium tartrate solution is recycled.
[0042] Through the above potassium removal treatment, the potassium removal rate in the rubidium-cesium salt crystals reaches 99.9%.
[0043] Step 3: Remove aluminum from the mixed solution.
[0044] The rubidium-cesium salt crystals are dissolved in deionized water, and a barium hydroxide solution or a calcium hydroxide solution is added while heating and stirring to control the pH of the reaction end point to be 6.5-8.5. After reaching the reaction end point, the temperature is kept for 10-60 minutes to precipitate aluminum in the form of aluminum hydroxide; the reaction mixture is centrifuged to obtain a clear liquid and a precipitated residue; the clear liquid is precisely filtered to obtain a purified rubidium-cesium salt solution and a filter residue.
[0045] First, the reaction mixture is centrifuged to remove the larger particle size flocs formed by flocculent aluminum hydroxide and calcium sulfate and / or barium sulfate. The centrifuged precipitate has a low water content and only carries a very small amount of rubidium and cesium, which can ensure a high yield of rubidium and cesium. At this time, the clear liquid still contains dispersed small-sized aluminum hydroxide suspended particles. Then, the clear liquid is filtered by precision filtration to achieve the purpose of secondary aluminum removal (secondary aluminum removal mainly removes small-sized aluminum hydroxide suspended particles, etc., and also removes small-sized calcium sulfate and / or barium sulfate). The obtained filtrate is a qualified impurity removal liquid, in which the aluminum ion content is reduced to below 0.002g / L.
[0046] The barium hydroxide solution or calcium hydroxide solution is prepared by dissolving analytically pure barium hydroxide or analytically pure calcium oxide in deionized water.
[0047] Through the above aluminum removal treatment, the aluminum removal rate in the mixed solution reaches 99.9%.
[0048] Step 4: Causticization and cesium extraction.
[0049] ① Add calcium hydroxide or barium hydroxide solution to the purified rubidium-cesium salt solution, heat and stir the solution while adding, the reaction temperature is 90-97°C, the pH at the reaction end point is controlled to be ≥13.0, and the solution is kept warm for 10-60 minutes after reaching the reaction end point, so that cesium is completely dissolved in the aqueous phase in the form of cesium hydroxide; after precise filtration, a causticized purified cesium-cesium-rubidium salt solution and barium slag or calcium slag are obtained; and cesium is extracted from the causticized purified cesium-cesium-rubidium salt solution.
[0050] ② Cesium extraction. The cesium extraction method is as follows: using a mixed solvent of t-BAMBP, diethylbenzene and kerosene as an extractant, extracting cesium from the causticized purified cesium rubidium salt solution to obtain a cesium extraction organic phase and a cesium extraction residual solution; washing the cesium extraction organic phase with water or a dilute alkaline solution (such as ammonia water) as a detergent to obtain a washing solution and a washed cesium extraction organic phase; after washing, stripping the cesium extraction organic phase with ammonium carbonate or oxalic acid as a stripping agent to obtain a cesium stripping solution. The cesium stripping solution is precisely filtered, evaporated, concentrated, crystallized, dried, calcined, recrystallized, and then dried to obtain high-purity cesium carbonate. If sulfuric acid or nitric acid is used as a stripping agent to strip the cesium extraction organic phase, the final product is cesium sulfate or cesium nitrate. Ammonia washing does not introduce metal ion impurities, and the washing effect is good.
[0051] Through the above cesium extraction process, the cesium removal rate in the purified rubidium-cesium salt solution reaches more than 99.9%.
[0052] Step 5: Carbonize the cesium extraction residual solution and purify it to obtain high-purity rubidium carbonate.
[0053] The dissolved substance in the cesium extraction residual solution is RbOH, and the remaining impurities are mainly trace amounts of Ba, Fe, Ca, and Mg metal ions. The specific method is: directly introduce high-purity CO into the cesium extraction residual solution 2 The pH value is kept constant (usually 8-9), filtered to obtain rubidium carbide solution and carbonate impurity salt (calcium, iron, magnesium, barium, etc.) precipitation; the rubidium carbide solution is precisely filtered, the filtrate is evaporated, concentrated, crystallized, dried, calcined, recrystallized, and then dried to obtain high-purity rubidium carbonate.
[0054] In the above steps, the precision filtration is a microporous filtration of 0.08-0.15 μm, preferably a microporous filtration of 0.10 μm.
[0055] The features and effects of the present invention are described below in conjunction with the preferred embodiments of the present invention.
[0056] Example 1
[0057] This embodiment provides a simplified process for preparing high-purity cesium salt and high-purity rubidium salt, and the steps are as follows:
[0058] (1) 300 g of potassium, rubidium and cesium mixed alum and deionized water were mixed and dissolved in a mass ratio of 1:4, heated to 75° C., and stirred continuously during the heating process to completely dissolve the rubidium and cesium alum to obtain a mixed solution containing potassium, rubidium and cesium.
[0059] (2): Add tartaric acid to a mixed solution containing potassium, rubidium and cesium, the molar ratio of the amount of tartaric acid added to the potassium in the mixed solution containing potassium, rubidium and cesium is controlled to be 0.35, heat to 60°C, and stir continuously during the heating process to dissolve the tartaric acid and react for 2 hours, then stand for 18 hours, cool to room temperature and recrystallize, centrifuge to obtain rubidium cesium alum crystals and potassium tartrate solution. The potassium content in the rubidium cesium alum crystals does not exceed 0.0030%.
[0060] (3): Dissolve the rubidium cesium alum crystals in deionized water, then slowly add 1 mol / L barium hydroxide solution. When the pH reaches 7.2, the reaction ends. Continue stirring for 0.5 hours to generate aluminum hydroxide and barium sulfate. Centrifuge the resulting mixture to obtain precipitate residue and clear liquid. Filter the clear liquid with a 0.1 μm microfiltration membrane to obtain a purified cesium rubidium salt solution and a barium slag precipitate. The aluminum content in the purified cesium rubidium salt solution is reduced to 0.002 g / L.
[0061] Among them, aluminum hydroxide flocs are adsorbed by barium slag and aggregated into large particles, which are separated by centrifugation; the centrifuged sediment has low water content and only carries a very small amount of rubidium and cesium, which can ensure a high yield of rubidium and cesium. At this time, the clear liquid also contains dispersed small-sized aluminum hydroxide suspended particles, and then the clear liquid is filtered by precision filtration to achieve the purpose of secondary aluminum removal.
[0062] (4): Add 1 mol / L barium hydroxide solution to the purified cesium rubidium salt solution, adjust the pH of the purified cesium rubidium salt solution to 13.2, and centrifuge to obtain a causticized purified cesium rubidium salt solution and barium slag. Use a mixed solvent of t-BAMBP, diethylbenzene and kerosene as an extractant to extract cesium from the causticized purified cesium rubidium salt solution to obtain a cesium extracted organic phase and a cesium extracted residual water, and the cesium content in the cesium extracted residual liquid is reduced to 0.001 g / L. Use ammonia water as a detergent to wash the cesium extracted organic phase to obtain a washing liquid and a washed cesium extracted organic phase. Then use ammonium carbonate as a stripping agent to strip the washed cesium extracted organic phase to obtain a cesium stripping solution and a lean organic phase. Rb / Cs in the cesium stripping solution is <0.002.
[0063] (5) Directly introduce high-purity CO into the cesium extraction residue 2 The pH is adjusted to 8 as the carbonization end point, and then filtered to obtain rubidium carbonization liquid and carbonate impurity salt (calcium, iron, magnesium, barium, etc.) precipitate.
[0064] (6): The cesium stripping solution and the rubidium carbonization solution are respectively finely filtered using a 0.1 μm microfiltration membrane. The filtered solutions are evaporated, concentrated, crystallized, dried, calcined, redissolved in deionized water, recrystallized, and dried to obtain high-purity cesium carbonate and high-purity rubidium carbonate products, respectively.
[0065] The purity of high-purity cesium carbonate is 99.9%, and the yield is 88.13%; the purity of high-purity rubidium carbonate is 99.9%, and the yield is 92.69%. The impurity metal ion content is: 0.003% cesium, 0.00012% sodium, 0.0012% potassium, 0.0002% iron, 0.0002% aluminum, and 0.003% calcium. According to the industry standard YS / T 789-2012 for rubidium carbonate and the industry standard YS / T756-2011 for cesium carbonate, the purity and impurity metal ion content of the cesium carbonate and rubidium carbonate products prepared in this embodiment meet the industry standards.
[0066] The comparison between this embodiment and the prior art is as follows: in terms of preparing high-purity rubidium salt, the equipment cost used in this embodiment is 1 / 150 of the prior art, and the reagent cost is 2 / 5 of the prior art (CO 2 The invention has the advantages of low cost, no wastewater treatment cost, and the process cycle is shortened to 1 / 10 of the existing process; the embodiment does not need to perform harmless treatment on the "lean organic phase after stripping rubidium", and no three wastes are generated. At the same time, the purity and recovery rate of the rubidium carbonate product prepared by the simplified process of the invention are not reduced.
[0067] Example 2
[0068] This embodiment provides a simplified process for preparing high-purity cesium salt and high-purity rubidium salt. Except for step (5), the other processing steps are the same as those in Example 1. In step (5), high-purity CO is directly introduced into the cesium extraction residue. 2 The pH is adjusted to 9 as the carbonization end point, and then filtered to obtain rubidium carbonization liquid and carbonate impurity salt (calcium, iron, magnesium, barium, etc.) precipitate.
[0069] The final purity of high-purity cesium carbonate is 99.9%, and the yield is 87.91%; the purity of high-purity rubidium carbonate is 99.9%, and the yield is 92.05%, and the impurity metal ion content thereof is: 0.003% of cesium, 0.00018% of sodium, 0.0014% of potassium, 0.0002% of iron, 0.0002% of aluminum, and 0.0029% of calcium. According to the industry standard YS / T 789-2012 for rubidium carbonate and the industry standard YS / T 756-2011 for cesium carbonate, the purity and impurity metal ion content of the cesium carbonate and rubidium carbonate products prepared in this embodiment meet the industry standards.
[0070] In summary, the present invention directly passes high-purity carbon dioxide through the cesium extraction residual solution and controls the carbonization endpoint. By only improving the method of extracting rubidium from the cesium extraction residual solution and retaining the cesium extraction and cesium stripping process of the cesium-rubidium mixed solution from which potassium and aluminum are removed, two high-purity products can be obtained while greatly reducing production costs, shortening the process cycle, and for specialized production enterprises of cesium salts and rubidium salts, the simplified process of the present invention can create very considerable economic benefits for rubidium salt and cesium salt production enterprises. Economic benefits are the most important technical contribution brought by the present invention.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A low-cost simplified process for preparing high-purity cesium salt and high-purity rubidium salt, characterized in that: It includes: S1, removing potassium and aluminum from a mixed solution containing rubidium, cesium and potassium to obtain a purified rubidium-cesium salt solution; the mixed solution containing rubidium, cesium and potassium is obtained by dissolving a mixed alum containing rubidium, cesium and potassium in deionized water; The potassium removal method comprises: adding tartaric acid to the mixed solution containing rubidium, cesium and potassium, wherein the molar ratio of tartaric acid to potassium in the mixed solution containing rubidium, cesium and potassium is 0.2-0.7, heating to a temperature of 50-95° C., reacting for 1-3 hours, standing for 12-24 hours, cooling for recrystallization, and centrifuging to precipitate rubidium salt and cesium salt in the form of crystals, and potassium tartrate is retained in the solution, thereby obtaining a potassium tartrate solution and rubidium cesium salt crystals with a potassium content of less than 0.0035%; The aluminum removal method comprises: dissolving rubidium-cesium salt crystals in deionized water, adding barium hydroxide solution or calcium hydroxide solution, heating and stirring the reaction while adding, controlling the pH value at the reaction end point to be 6.5-8.5, and keeping the temperature for 10-60 minutes after reaching the reaction end point, so that aluminum precipitates in the form of aluminum hydroxide; centrifuging the reaction mixture to obtain a clear liquid and a precipitated residue; finely filtering the clear liquid to obtain a purified rubidium-cesium salt solution and a filter residue; the content of aluminum ions in the purified rubidium-cesium salt solution is reduced to below 0.002 g / L; S2, extracting cesium from the purified rubidium-cesium salt solution to obtain a cesium-extracted organic phase and a cesium-extracted residual solution; washing the cesium-extracted organic phase; stripping the washed cesium-extracted organic phase with a stripping agent to obtain a cesium stripping solution; the stripping agent is ammonium carbonate or oxalic acid; accurately filtering the cesium stripping solution, sequentially evaporating, concentrating, crystallizing, drying, calcining, recrystallizing, and then drying to obtain high-purity cesium carbonate with a purity of more than 99.9%; S3, the dissolved substance in the cesium extraction residual solution is RbOH, and the other impurities are mainly trace metal ions of Ba, Fe, Ca and Mg; high-purity CO2 is introduced into the cesium extraction residual solution until the pH reaches 8-9 and does not change, and filtered to obtain rubidium carbide solution and carbonate impurity salt precipitation; the rubidium carbide solution is precisely filtered, and the filtrate is the purified rubidium carbide solution, which is evaporated, concentrated and crystallized, dried, calcined, redissolved in deionized water, evaporated, concentrated and crystallized again to obtain high-purity rubidium carbonate, and the purity of the high-purity rubidium carbonate is more than 99.9%; the precise filtration is a microporous filtration of 0.08-0.15μm.
2. The low-cost simplified process according to claim 1, characterized in that: In S2, before cesium extraction, the pH of the purified rubidium-cesium salt solution is adjusted to alkaline, and then finely filtered to obtain a causticized purified cesium-cesium salt solution and a filter residue; and cesium extraction is performed on the causticized purified cesium-cesium salt solution.
3. The low-cost simplified process according to claim 1, characterized in that: In S2, before cesium extraction, calcium hydroxide or barium hydroxide solution is added to the purified rubidium-cesium salt solution, while heating and stirring the reaction, the reaction temperature is 90-97°C, the reaction end point pH is controlled to be ≥13.0, and after reaching the reaction end point, the temperature is kept for 10min-60min to make cesium completely dissolved in the aqueous phase in the form of cesium hydroxide; after precise filtration, a causticized purified cesium rubidium salt solution and barium slag or calcium slag are obtained; and cesium extraction is performed on the causticized purified cesium rubidium salt solution.
4. The low-cost simplified process according to claim 2 or 3, characterized in that: In S2, the cesium extraction method is: using a mixed solvent of t-BAMBP, diethylbenzene and kerosene as an extractant, extracting cesium from a causticized purified cesium rubidium salt solution to obtain a cesium extracted organic phase and a cesium extracted residual solution; washing the cesium extracted organic phase with water or a dilute alkali aqueous solution as a detergent to obtain a washing liquid and a washed cesium extracted organic phase; after washing, stripping the cesium extracted organic phase with ammonium carbonate or oxalic acid as a stripping agent to obtain a cesium stripping solution, and precisely filtering the cesium stripping solution, and sequentially evaporating, concentrating, crystallizing, drying, calcining, recrystallizing and drying to obtain high-purity cesium carbonate.
5. The low-cost simplified process according to claim 1, characterized in that: After step S1, the removal rate of potassium and aluminum in the mixed solution containing rubidium, cesium and potassium reaches more than 99.9%; After the treatment in step S2, the cesium removal rate in the purified rubidium-cesium salt solution reaches more than 99.9%.