A kind of organic silicon waterproofing agent and preparation method thereof
Through the silicone waterproofing agent and high-pressure homogenization process with specific component ratios, the problem of high VOC and lack of reactivity in the prior art is solved, and the waterproofing effect with low VOC and high durability is achieved, which is suitable for multiple Application of substrates.
Patent Information
- Application Number
- CN202310501541.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-04
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-04
AI Technical Summary
The existing silicone waterproofing agent has high volatile organic content and lacks reactivity and permeability, which cannot meet the long-term waterproofing needs of substrates.
Silicone waterproofing agents in specific component proportions, including silane crosslinking agents, silane oligomers, Q-type resins, surfactants, additives and preservatives, are prepared by high-pressure homogenization process to form an emulsion containing active groups. , suitable for construction, fabric, leather and other fields.
It achieves a VOC content of less than 50g/L, improves waterproof durability and permeability, and is suitable for a wide range of surface coating applications, with good waterproof performance and stability.
Smart Images

Figure BDA0004213991230000121 
Figure BDA0004213991230000131 
Figure BDA0004213991230000132
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fine chemical preparations, and more specifically to an organosilicon waterproofing agent and a preparation method thereof. Background Art
[0002] Buildings, fabrics, leather, etc. are easily degraded by the physical, chemical and microbial effects of the use environment, which greatly reduces their performance and durability, or even destroys them. Silicone includes silane, polysiloxane such as silicone oil and silicone resin, which is the preferred material for waterproofing. It has been widely used at home and abroad. Whether it is fabric, leather or building materials, they can be treated with silicone waterproofing agents to make them waterproof.
[0003] Silicone waterproofing agent can not only effectively prevent and reduce the erosion of water on the substrate, but also the protective film formed does not affect the outward diffusion of internal moisture; its surface tension is low, which can reduce the surface energy of the substrate, and has good hydrophobicity and anti-fouling properties. The existing silicon hydroxyl groups can easily condense with themselves or the hydroxyl groups in the substrate to form chemical bonds under certain conditions, and have high adhesion and bonding strength. It has good resistance to environmental factors such as ultraviolet radiation, heat, corrosive chemicals and microorganisms. At the same time, it is easy to use and cost-effective.
[0004] Silicone water repellent compounds initially used silicone resins in solvents and methylsilanol salts, and then used siloxane and silane-based products in solvents. The new generation of water repellents are generally water-based for environmental reasons and ease of use. The active ingredients of water-based water repellents include siloxanes, silicone resins or silanes (and combinations thereof). Water repellents with water as the dispersion medium overcome the toxicity, volatility and flammability of solvent-based water repellents.
[0005] For example, US5074912 discloses a waterproofing agent composition for treating porous substrates with a silicone-containing emulsion, however, the volatile organic content (VOC) of the product is higher than 100 g / L, but an emulsion with a VOC of less than 100 g / L or even less than 50 g / L is desired. WO200813423A1 describes an organosilicon emulsion for applying waterproofing, which contains phenyl silsesquioxane and has a VOC content of less than 100 g / L; however, the waterproofing agent emulsion lacks reactivity and penetration depth and cannot meet the long-term waterproofing requirements of the substrate. Summary of the invention
[0006] In view of this, the object of the present invention is to provide an organosilicon waterproofing agent and a preparation method thereof. The organosilicon waterproofing agent provided by the present invention has a low VOC content, which meets the requirement that the VOC is less than 50 g / L, and contains active groups (such as hydroxyl groups), which can further react with the substrate, which is beneficial to improve the durability of waterproofing. The organosilicon waterproofing agent is suitable for use as a surface coating layer in a wide range of applications in the fields of construction, fabrics, leather, coatings, etc. for waterproofing.
[0007] The present invention provides an organosilicon waterproofing agent, which is prepared from the following raw materials:
[0008] Silane crosslinking agent 1wt% to 5wt%;
[0009] Silane oligomer 20wt% to 50wt%;
[0010] Q-type resin 5wt% to 20wt%;
[0011] Surfactant 2wt%~10wt%;
[0012] Additives 0.5wt%~2wt%;
[0013] Preservative 0.1wt%~1wt%;
[0014] Water balance.
[0015] Preferably, the general structural formula of the silane crosslinking agent is R1SiD3, wherein the D group is a hydrolyzable group, and the R group is one or more of a hydrocarbon group and an aromatic group having 3 to 20 carbon atoms.
[0016] Preferably, the general structural formula of the silane oligomer is (R 1 3SiO 0.5 ) x (R 2 SiO 1.5 ) m (R 3 2SiO) n (O 0.5 R') t ; wherein x is 0 to 100, m is 5 to 200, n is 0 to 200, and t+x=m+2; R' is one of the hydrocarbon groups having 1 to 10 carbon atoms or H, R 1 , R 3 is independently selected from one or more of a hydrocarbon group having 1 to 10 carbon atoms, a halogenated hydrocarbon group having 3 to 10 carbon atoms, and an aryl group, R 2 It is one or more of a hydrocarbon group having 1 to 10 carbon atoms, an amino hydrocarbon group having 1 to 10 carbon atoms, and an aryl group.
[0017] Preferably, the Q-type resin is MQ silicone resin and / or water-soluble silica sol; wherein the MQ silicone resin is composed of linked M units R3SiO 0.5 and link Q unit SiO 4 / 2The silicone resin has an M / Q ratio of 0.5 to 1.5, and the R groups in the M units are the same or different, including one or more of hydrogen atoms, hydroxyl groups, monovalent substituted or unsubstituted hydrocarbon groups with 1 to 20 carbon atoms, and halogenated hydrocarbon groups with 3 to 20 carbon atoms. The content of hydroxyl groups in the R groups is 0.5% to 1.5%. The water-soluble silica sol is a colloidal solution of a multi-molecular polymer of silicic acid, in which the silicon dioxide content is 20% to 50% and the particle size is 5nm to 30nm.
[0018] Preferably, the surfactant is a cationic surfactant, an anionic surfactant, a nonionic surfactant or a composite ionic surfactant; wherein the cationic surfactant is selected from one or more of fatty amine salts, ethanolamine salts, and polyethylene polyamine salts to form a cationic emulsion; the anionic surfactant is selected from one or more of anionic polyacrylamide, fatty acid salts, sulfonates, sulfate esters, and phosphate esters to form an anionic emulsion; the nonionic surfactant is selected from one or more of Span series, Tween series, polyethylene glycol fatty acid esters, fatty alcohol polyoxyethylene ethers, alkylphenol polyoxyethylene ethers, isomeric alcohol polyoxyethylene ethers, and nonylphenol polyoxyethylene ethers to form a nonionic emulsion; the composite ionic surfactant is a mixture of a nonionic emulsifier and an ionic emulsifier used as an emulsifier to form a composite ionic emulsion.
[0019] Preferably, the auxiliary agent is selected from one or more of ethylene glycol, propylene glycol, propylene glycol butyl ether, ethylene glycol butyl ether, and a defoaming agent.
[0020] Preferably, the preservative is selected from one or more of phenoxyethanol, copper nitrate, copper sulfate, dimethyloldimethylhydantoin, and isothiazolinone.
[0021] The present invention also provides a method for preparing the organosilicon waterproofing agent described in the above technical solution, comprising the following steps:
[0022] a) mixing a silane crosslinking agent, a silane oligomer, a Q-type resin and a surfactant, and then adding water dropwise until a phase inversion is achieved to obtain a crude emulsion;
[0023] b) homogenizing the crude emulsion obtained in step a) under high pressure, adding an auxiliary agent and a preservative, and stirring evenly to obtain an organosilicon waterproofing agent.
[0024] Preferably, the mixing process in step a) is carried out in a stirred reactor; the mixing temperature is 10°C to 40°C, the stirring speed is 800r / min to 2000r / min, and the time is 30min to 120min.
[0025] Preferably, the pressure of the high-pressure homogenization in step b) is 300 bar to 1200 bar.
[0026] The present invention provides an organosilicon waterproofing agent, which is prepared from the following raw materials: 1wt% to 5wt% of silane crosslinking agent; 20wt% to 50wt% of silane oligomer; 5wt% to 20wt% of Q-type resin; 2wt% to 10wt% of surfactant; 0.5wt% to 2wt% of auxiliary agent; 0.1wt% to 1wt% of preservative; and water balance. Compared with the prior art, the organosilicon waterproofing agent provided by the present invention adopts specific components with specific contents to achieve better overall interaction, has a low VOC content, and meets the requirement that VOC is less than 50g / L. At the same time, it contains active groups (such as hydroxyl groups) that can further react with substrates, which is beneficial to improving the durability of waterproofing. It is suitable for being widely used as a surface coating layer in the fields of construction, fabrics, leather, coatings, etc. for waterproofing.
[0027] In addition, the preparation method provided by the present invention has a simple and easy process and is convenient for scale-up production. Meanwhile, the reaction conditions are mild and easy to control. The quality of the prepared product is stable and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 A schematic diagram of the waterproof application of the organosilicon waterproofing agent provided in an embodiment of the present invention on a building substrate. DETAILED DESCRIPTION
[0029] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] The present invention provides an organosilicon waterproofing agent, which is prepared from the following raw materials:
[0031] Silane crosslinking agent 1wt% to 5wt%;
[0032] Silane oligomer 20wt% to 50wt%;
[0033] Q-type resin 5wt% to 20wt%;
[0034] Surfactant 2wt%~10wt%;
[0035] Additives 0.5wt%~2wt%;
[0036] Preservative 0.1wt%~1wt%;
[0037] Water balance.
[0038] In the present invention, the organosilicon waterproofing agent is prepared from a silane crosslinking agent, a silane oligomer, a Q-type resin, a surfactant, an auxiliary agent, a preservative and water. The present invention has no particular restrictions on the sources of the silane crosslinking agent, the silane oligomer, the Q-type resin, the surfactant, the auxiliary agent and the preservative, and commercial products well known to those skilled in the art can be used; the water can be deionized water well known to those skilled in the art.
[0039] In the present invention, the general structural formula of the silane crosslinker is preferably R1SiD3; wherein the D group is preferably a hydrolyzable group, such as an alkoxy (methoxy), acyloxy or oxime group, and the R group is preferably a combination of one or more hydrocarbon groups and aromatic groups with a carbon number of 3 to 20, more preferably an octyl group, a butyl group or a phenyl group.
[0040] In the present invention, the general structural formula of the silane oligomer is preferably (R 1 3SiO 0.5 ) x (R 2 SiO 1.5 ) m (R 3 2SiO) n (O 0.5 R') t ; wherein x is preferably 0 to 100, more preferably 20 to 100, m is preferably 5 to 200, more preferably 80 to 200, n is preferably 0 to 200, more preferably 30 to 200, and t+x=m+2; R' is preferably one of the hydrocarbon groups having 1 to 10 carbon atoms or H, more preferably one of the hydrocarbon groups having 3 to 10 carbon atoms or H, and even more preferably methyl, ethyl, pentyl or H; R 1 Preferably, it is selected from one or more combinations of hydrocarbon groups having 1 to 10 carbon atoms, halogenated hydrocarbon groups having 3 to 10 carbon atoms, and aryl groups, and more preferably, it is methyl or ethyl; R 2 Preferably, it is a hydrocarbon group having 1 to 10 carbon atoms, an amino hydrocarbon group having 1 to 10 carbon atoms, or one or more combinations of an aryl group, and more preferably, it is an aminopropyl group, an octyl group, a phenyl group, or an aminoethyl group; R 3 It is preferably selected from one or more combinations of hydrocarbon groups having 1 to 10 carbon atoms, halogenated hydrocarbon groups having 3 to 10 carbon atoms, and aryl groups, and more preferably methyl, phenyl, or both methyl and trifluoropropyl groups.
[0041] In the present invention, the Q-type resin is preferably MQ silicone resin and / or water-soluble silica sol, more preferably MQ silicone resin or water-soluble silica sol; wherein the MQ silicone resin is preferably composed of linked M units R3SiO 0.5 and link Q unit SiO 4 / 2The silicone resin composed of the above-mentioned components has an M / Q ratio of preferably 0.5-1.5, which can be limited to 0.5, 0.6, 1, 1.2, and 1.5. The R groups in the M units are the same or different, and preferably include one or more of hydrogen atoms, hydroxyl groups, monovalent substituted or unsubstituted hydrocarbon groups with 1 to 20 carbon atoms, and halogenated hydrocarbon groups with 3 to 20 carbon atoms, and more preferably methyl and hydroxyl groups, or ethyl and hydroxyl groups, or H and hydroxyl groups, or methyl, trifluoropropyl and hydroxyl groups. The content of hydroxyl groups in the R groups is preferably 0.5%-1.5%, which can be limited to 0.5%, 1%, 1.2%, and 1.5%. The water-soluble silica sol is preferably a colloidal solution of a multimolecular polymer of silicic acid, in which the silicon dioxide content is preferably 20%-50%, and the particle size is preferably 5nm-30nm, and more preferably 5nm-20nm.
[0042] In the present invention, the surfactant is preferably a cationic surfactant, an anionic surfactant, a nonionic surfactant or a composite ionic surfactant; wherein the cationic surfactant is preferably selected from one or more combinations of fatty amine salts, ethanolamine salts, and polyethylene polyamine salts to prepare a cationic emulsion; the anionic surfactant is preferably selected from one or more combinations of anionic polyacrylamide, fatty acid salts, sulfonates, sulfate esters, and phosphate esters to prepare anionic emulsions; the nonionic surfactant is preferably selected from Span series, Tween series, polyethylene glycol fatty acid esters, fatty alcohol polyoxyethylene ethers, alkylphenol polyoxyethylene ethers, isomerized One or more combinations of alcohol polyoxyethylene ether and nonylphenol polyoxyethylene ether are used to prepare a nonionic emulsion; the composite ionic surfactant is preferably a mixture of a nonionic emulsifier and an ionic emulsifier used as an emulsifier to prepare a composite ionic emulsion; more preferably: nonylphenol polyoxyethylene ether and dodecylbenzenesulfonic acid triethanolamine salt, or isomeric alcohol polyoxyethylene ether, or fatty acid triethanolamine salt and hexadecylbenzenesulfonic acid triethanolamine salt, or alkylphenol polyoxyethylene ether, or stearic acid triethanolamine salt, or sodium dodecylbenzenesulfonate, or fatty alcohol polyoxyethylene ether and 1-dodecylamine acetate, or fatty alcohol polyoxyethylene ether and sodium dodecylbenzenesulfonate.
[0043] In the present invention, the auxiliary agent is preferably selected from one or more combinations of ethylene glycol, propylene glycol, propylene glycol butyl ether, ethylene glycol butyl ether, and defoaming agent, and more preferably one or two of ethylene glycol, propylene glycol, ethylene glycol butyl ether, and defoaming agent.
[0044] In the present invention, the preservative is preferably selected from one or more combinations of phenoxyethanol, copper nitrate, copper sulfate, dimethyloldimethylhydantoin, and isothiazolinone, more preferably phenoxyethanol, dimethyloldimethylhydantoin or isothiazolinone.
[0045] The organosilicon waterproofing agent provided by the present invention adopts specific components at specific contents to achieve good overall interaction, low VOC content, and meets the requirement of VOC less than 50g / L. It also contains active groups (such as hydroxyl groups) that can further react with the substrate, which is beneficial to improve the durability of waterproofing. It is suitable for use as a surface coating layer in a wide range of applications in the fields of construction, fabrics, leather, coatings, etc. for waterproofing; for example, a schematic diagram of waterproofing application on a building substrate can be seen in Figure 1 shown.
[0046] The present invention also provides a method for preparing the organosilicon waterproofing agent described in the above technical solution, comprising the following steps:
[0047] a) mixing a silane crosslinking agent, a silane oligomer, a Q-type resin and a surfactant, and then adding water dropwise until a phase inversion is achieved to obtain a crude emulsion;
[0048] b) homogenizing the crude emulsion obtained in step a) under high pressure, adding an auxiliary agent and a preservative, and stirring evenly to obtain an organosilicon waterproofing agent.
[0049] The present invention first mixes a silane crosslinking agent, a silane oligomer, a Q-type resin, and a surfactant, and then drips water until a phase inversion is achieved to obtain a crude emulsion. In the present invention, the silane crosslinking agent, the silane oligomer, the Q-type resin, the surfactant, and the water are the same as those in the above technical solution, and are not described in detail herein.
[0050] In the present invention, the mixing process is preferably carried out in a stirred reactor; the mixing temperature is preferably 10°C to 40°C, specifically 10°C, 20°C, 25°C, 30°C, 40°C; the stirring speed is preferably 800r / min to 2000r / min, specifically 800r / min, 1200r / min, 1500r / min, 2000r / min; the time is preferably 30min to 120min, specifically 30min, 60min, 90min, 120min.
[0051] After obtaining the crude emulsion, the present invention homogenizes the obtained crude emulsion under high pressure, adds auxiliary agents and preservatives, and stirs evenly to obtain an organosilicon waterproofing agent. In the present invention, the auxiliary agents and preservatives are the same as those in the above technical solution, and are not described in detail here.
[0052] In the present invention, the pressure of the high-pressure homogenization is preferably 300 bar to 1200 bar, and can be specifically limited to 300 bar, 450 bar, 500 bar, 800 bar, and 1200 bar.
[0053] The preparation method provided by the present invention comprises the following steps: firstly adding a silane crosslinking agent, a silane oligomer, a Q-type resin and a surfactant into a stirring reactor, stirring and mixing at a certain temperature for a certain time, slowly adding water dropwise until a phase transition is performed to obtain a crude emulsion; then the crude emulsion is homogenized by high pressure, an auxiliary agent and a preservative are added, and the mixture is stirred evenly to obtain an organosilicon waterproofing agent; the VOC content of the waterproofing agent emulsion is low, and the requirement of VOC being less than 50 g / L is met; the prepared waterproofing agent emulsion contains active groups (such as hydroxyl groups), which can further react with a substrate, and are beneficial to improving the durability of waterproofing; the organosilicon waterproofing agent emulsion has a wide range of applications, and can be widely used as a surface coating layer in the fields of construction, fabrics, leather, coatings, etc. for waterproofing.
[0054] At the same time, the preparation method provided by the present invention has a simple and easy process and is convenient for scale-up production. At the same time, the reaction conditions are mild and easy to control. The quality of the prepared product is stable and has broad application prospects.
[0055] The present invention provides an organosilicon waterproofing agent, which is prepared from the following raw materials: 1wt% to 5wt% of silane crosslinking agent; 20wt% to 50wt% of silane oligomer; 5wt% to 20wt% of Q-type resin; 2wt% to 10wt% of surfactant; 0.5wt% to 2wt% of auxiliary agent; 0.1wt% to 1wt% of preservative; and water balance. Compared with the prior art, the organosilicon waterproofing agent provided by the present invention adopts specific components with specific contents to achieve better overall interaction, has a low VOC content, and meets the requirement that VOC is less than 50g / L. At the same time, it contains active groups (such as hydroxyl groups) that can further react with substrates, which is beneficial to improving the durability of waterproofing. It is suitable for being widely used as a surface coating layer in the fields of construction, fabrics, leather, coatings, etc. for waterproofing.
[0056] In addition, the preparation method provided by the present invention has a simple and easy process and is convenient for scale-up production. Meanwhile, the reaction conditions are mild and easy to control. The quality of the prepared product is stable and has broad application prospects.
[0057] In order to further illustrate the present invention, the following examples are provided for detailed description. In the following examples / comparative examples of the present invention, all reagents used were of analytical grade and commercially available unless otherwise specified.
[0058] Example 1
[0059] Accurately weigh 5 g of silane crosslinker (D group is methoxy, R group is octyl), silane oligomer (x = 50, m = 80, n = 150, t = 32, R' is H, R 1 , R 3 is methyl, R 2The mixture was stirred for 30 min at 25 °C (stirring speed: 1500 r / min), and 110 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 450 bar), 2 g of an auxiliary agent (ethylene glycol) and 1 g of a preservative (phenoxyethanol) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0060] Example 2
[0061] Accurately weigh 8 g of silane crosslinker (D group is acyloxy, R group is butyl) and silane oligomer (x=20, m=150, n=60, t=132, R' is methyl, R 1 Ethyl, R 2 For octyl, R 3 The mixture was stirred for 60 min at 40 °C (stirring speed: 2000 r / min), and 114 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 450 bar), 1 g of an auxiliary agent (ethylene glycol butyl ether) and 1 g of a preservative (isothiazolinone) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0062] Example 3
[0063] Accurately weigh 10 g of silane crosslinker (D group is oxime group, R group is octyl group), silane oligomer (x=100, m=200, n=100, t=102, R' is pentyl group, R 1 , R 3 is methyl, R 2 The mixture was stirred for 120 min at 20 °C (stirring speed: 800 r / min), and 85.8 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 1200 bar), 4 g of an auxiliary agent (ethylene glycol butyl ether) and 0.2 g of a preservative (isothiazolinone) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0064] Example 4
[0065] Accurately weigh 2 g of silane crosslinker (D group is oxime group, R group is phenyl group), silane oligomer (x=0, m=200, n=0, t=202, R' is pentyl group, R 2 The mixture was stirred for 60 min at 30°C (stirring speed: 1200 r / min), and 75.8 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 300 bar), 4 g of an auxiliary agent (ethylene glycol butyl ether) and 0.2 g of a preservative (isothiazolinone) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0066] Example 5
[0067] Accurately weigh 10 g of silane crosslinker (D group is acyloxy, R group is octyl), silane oligomer (x=50, m=100, n=200, t=52, R' is ethyl, R 1 , R 3 is methyl, R 2 The mixture was stirred for 60 min at 10°C (stirring speed: 1500 r / min), and 92.4 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 800 bar), 4 g of an auxiliary agent (ethylene glycol) and 1.6 g of a preservative (dihydroxymethyl dimethyl hydantoin) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0068] Example 6
[0069] Accurately weigh 5 g of silane crosslinker (D group is methoxy, R group is phenyl), silane oligomer (x=20, m=80, n=0, t=62, R' group is methyl, R 1 is methyl, R 2 80 g of octyl) 25 g of water-soluble silica sol (silicon dioxide content 20%, particle size 20 nm) and 12 g of alkylphenol polyoxyethylene ether are added into a stirred reactor, stirred and mixed at 25°C for 90 min (stirring speed: 800 r / min), 76.5 g of water is slowly added dropwise until the phase is inverted to obtain a crude emulsion; after the crude emulsion is homogenized under high pressure (homogenization pressure: 500 bar), 1 g of an auxiliary agent (defoaming agent) and 0.5 g of a preservative (dihydroxymethyl dimethyl hydantoin) are added, and stirred evenly to obtain a silicone waterproofing agent emulsion.
[0070] Example 7
[0071] Accurately weigh 3 g of silane crosslinker (D group is acyloxy, R group is butyl) and silane oligomer (x = 0, m = 100, n = 30, t = 102, R' group is H, R 2 is aminopropyl, R 3 The mixture was stirred for 30 min at 40 °C (stirring speed: 1200 r / min), and 98 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 800 bar), 4 g of an auxiliary agent (propylene glycol) and 1 g of a preservative (phenoxyethanol) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0072] Example 8
[0073] Accurately weigh 2 g of silane crosslinker (D group is oxime group, R group is phenyl group), silane oligomer (x=0, m=200, n=0, t=202, R' is pentyl group, R 2 The mixture was stirred for 60 min at 30 °C (stirring speed: 1200 r / min), and 77.8 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 300 bar), 1 g of an auxiliary agent (ethylene glycol butyl ether), 1 g of an auxiliary agent (defoaming agent) and 0.2 g of a preservative (isothiazolinone) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0074] Example 9
[0075] Accurately weigh 2 g of silane crosslinker (D group is oxime group, R group is phenyl group), silane oligomer (x=50, m=200, n=50, t=152, R' is pentyl group, R 1 , R 3 is methyl, R 2 The mixture was stirred for 60 min at 30 °C (stirring speed: 1200 r / min), and 75.8 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion; after the crude emulsion was homogenized under high pressure (homogenizing pressure: 300 bar), 4 g of an auxiliary agent (ethylene glycol butyl ether) and 0.2 g of a preservative (isothiazolinone) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0076] Example 10
[0077] Accurately weigh 5 g of silane crosslinker (D group is methoxy, R group is octyl), silane oligomer (x = 50, m = 80, n = 150, t = 32, R' is H, R 1 , R 3 is methyl, R 2 The mixture was stirred for 30 min at 25 °C (stirring speed: 1500 r / min), and 110 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 450 bar), 2 g of an auxiliary agent (ethylene glycol) and 1 g of a preservative (phenoxyethanol) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0078] Embodiment 11
[0079] Accurately weigh 10 g of silane crosslinker (D group is methoxy, R group is octyl), silane oligomer (x=50, m=80, n=150, t=32, R' is H, R 1 , R 3 is methyl, R 2 The mixture was stirred for 30 min at 25 °C (stirring speed: 1500 r / min), and 105 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 450 bar), 2 g of an auxiliary agent (ethylene glycol) and 1 g of a preservative (phenoxyethanol) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0080] Example 12
[0081] Accurately weigh 5 g of silane crosslinker (D group is methoxy, R group is octyl), silane oligomer (x = 50, m = 80, n = 150, t = 32, R' is H, R 1 , R 3 is methyl, R 2The mixture was stirred for 120 min at 25 °C (stirring speed: 1500 r / min), and 110 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 450 bar), 2 g of an auxiliary agent (ethylene glycol) and 1 g of a preservative (phenoxyethanol) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0082] Embodiment 13
[0083] Accurately weigh 5 g of silane crosslinker (D group is methoxy, R group is octyl), silane oligomer (x = 50, m = 80, n = 150, t = 32, R' is H, R 1 , R 3 is methyl, R 2 The mixture was stirred for 30 min at 25 °C (stirring speed: 1500 r / min), and 310 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion; after the crude emulsion was homogenized under high pressure (homogenizing pressure: 450 bar), 2 g of an auxiliary agent (ethylene glycol) and 1 g of a preservative (phenoxyethanol) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0084] Comparative Example 1
[0085] The difference between this comparative example and Example 3 is the presence or absence of a silane crosslinking agent
[0086] Accurately weigh the silane oligomer (x = 100, m = 200, n = 100, t = 102, R' is pentyl, R 1 , R 3 is methyl, R 2 The mixture was stirred for 120 min at 20 °C (stirring speed: 800 r / min), and 85.8 g of water was slowly added dropwise until the phase was inverted to obtain a crude emulsion. After the crude emulsion was homogenized under high pressure (homogenizing pressure: 1200 bar), 4 g of an auxiliary agent (ethylene glycol butyl ether) and 0.2 g of a preservative (isothiazolinone) were added, and the mixture was stirred evenly to obtain a silicone waterproofing agent emulsion.
[0087] Comparative Example 2
[0088] The difference between this comparative example and Example 3 is the presence or absence of silane oligomer
[0089] Accurately weigh 10 g of a silane crosslinker (the D group is an oxime group, and the R group is an octyl group), 40 g of an MQ resin (M / Q=1, the R group on the M unit is H and a hydroxyl group, and the hydroxyl content is 1.5%), and 20 g of isomeric alcohol polyoxyethylene ether, and add them into a stirred reactor. Stir and mix at a temperature of 20°C for 120 min (stirring speed: 800 r / min), and slowly add 85.8 g of water dropwise until the phase is inverted to obtain a crude emulsion; after the crude emulsion is homogenized under high pressure (homogenization pressure: 1200 bar), 4 g of an auxiliary agent (ethylene glycol butyl ether) and 0.2 g of a preservative (isothiazolinone) are added, and the mixture is stirred evenly to obtain a silicone waterproofing agent emulsion.
[0090] The various properties of the organosilicon waterproofing agent emulsions provided in Examples 1 to 13 and Comparative Examples 1 to 2 were tested, specifically including:
[0091] Test Example 1
[0092] Physical and chemical properties:
[0093] The physical and chemical properties of the organosilicon emulsions obtained in Examples 1 to 13 and Comparative Examples 1 to 2 were tested according to appearance, stability (GB / T 20623-2006) and VOC content (GB 18582-2020). The results are shown in Table 1.
[0094] Table 1 Physical and chemical properties test results of Examples 1 to 13 and Comparative Examples 1 to 2
[0095]
[0096]
[0097] Test Example 2
[0098] The application performance test of the organosilicon waterproofing agents prepared in Examples 1 to 13 and Comparative Examples 1 to 2 was carried out according to the water absorption ratio, penetration depth and alkali resistance (JC / T2235-2014). The test results are shown in Table 2.
[0099] Table 2 Application performance test results of Examples 1 to 13 and Comparative Examples 1 to 2
[0100]
[0101]
[0102] Test Example 3
[0103] The application durability test was conducted on the organosilicon waterproofing agents prepared in Examples 1 to 13 and Comparative Examples 1 to 2 according to the permeability (JC / T 902-2002). The test results are shown in Table 3.
[0104] Table 3 Durability test results of Examples 1 to 13 and Comparative Examples 1 to 2
[0105]
[0106]
[0107] As shown in Table 1, the organosilicon waterproofing agents of Examples 1 to 13 and Comparative Example 1 have lower VOC values and better stability. Compared with Example 3, the freeze-thaw stability, storage stability and mechanical stability of Comparative Example 2 are poor. As shown in Table 2, the organosilicon waterproofing agents of Examples 1 to 13 have higher permeability, good waterproof performance and alkali resistance because they form point-shaped, linear and branch-shaped three-dimensional space structure waterproofing films. Compared with Example 3, Comparative Example 1 has no silane cross-linking agent, and the cross-linking ability of the polysiloxane molecular chain and the hydrophilic group on the substrate is insufficient. Its waterproof product has poor permeability and poor alkali resistance. Comparative Example 2 has no silane oligomers and cannot form a three-dimensional space structure waterproofing film, and its waterproofness and alkali resistance are poor. As shown in Table 3, the organosilicon waterproofing agents of Examples 1 to 13 have better resistance to high and low temperatures, ultraviolet rays and acid and alkali. Compared with Example 3, the waterproof performance of Comparative Examples 1 to 2 after being treated with high temperature, low temperature, ultraviolet rays, acid and alkali has been significantly reduced.
[0108] In summary, the present invention has the following beneficial effects:
[0109] (1) The silicone waterproofing agent emulsion contains active groups that can combine with the hydroxyl groups in the substrate to form a directional hydrophobic film several nanometers thick without affecting the appearance of the substrate;
[0110] (2) The VOC content of the silicone waterproofing agent is low, meeting the requirement of VOC less than 50g / L;
[0111] (3) The synergistic effect of Q-type silicone resin, silane oligomer and silane crosslinker forms a three-dimensional waterproof membrane with dot, line and branch structures on the surface of the substrate, which is beneficial to the vertical orientation of the carbon chain relative to the Si-O-Si main chain and the aggregation and hydrophobic effect between the chains, more effectively hindering the diffusion of water into the structure and greatly improving the waterproof performance;
[0112] (4) The introduction of silane crosslinking agent helps the polysiloxane molecular chain to better crosslink with the hydrophilic groups on the substrate, thereby improving the waterproof durability of the substrate;
[0113] (5) The deposition of silane oligomers and Q-type resins on the surface of the substrate avoids the defects of traditional waterproofing agents due to their strong penetration and insufficient surface coating thickness, greatly enhancing the waterproofing effect and durability;
[0114] (6) Silicone waterproofing agents have good water-repellent and waterproofing effects and show excellent performance in application fields such as construction, fabrics, leather, and coatings.
[0115] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A silicone waterproofing agent, characterized in that: Prepared from the following raw materials: Silane crosslinking agent 1wt%~5wt%; Silane oligomer 20wt%~50wt%; Q-type resin 5wt%~20wt%; Surfactant 2wt%~10wt%; Additives 0.5wt%~2wt%; Preservatives 0.1wt%~1wt%; Water balance; The general structural formula of the silane oligomer is (R 1 3SiO 0.5 ) x (R 2 SiO 1.5 ) m (R 3 2SiO) n (O 0.5 R') t ; wherein x is 0 to 100, m is 5 to 200, n is 0 to 200, and t+x=m+2; R' is one of the hydrocarbon groups having 1 to 10 carbon atoms or H, R 1 , R 3 is independently selected from one or more of a hydrocarbon group having 1 to 10 carbon atoms, a halogenated hydrocarbon group having 3 to 10 carbon atoms, and an aryl group, R 2 is one or more of a hydrocarbon group having 1 to 10 carbon atoms, an amino hydrocarbon group having 1 to 10 carbon atoms, and an aryl group; The Q-type resin is MQ silicone resin and / or water-soluble silica sol; wherein the MQ silicone resin is composed of linked M units R3SiO 0.5 and link Q unit SiO 4 / 2 The silicone resin has an M / Q ratio of 0.5-1.5, the R groups in the M units are the same or different, including one or more of hydrogen atoms, hydroxyl groups, monovalent substituted or unsubstituted hydrocarbon groups with 1-20 carbon atoms, and halogenated hydrocarbon groups with 3-20 carbon atoms, and the content of hydroxyl groups in the R groups is 0.5%-1.5%; the water-soluble silica sol is a colloidal solution of a multi-molecular polymer of silicic acid, in which the silicon dioxide content is 20%-50% and the particle size is 5nm-30nm.
2. The organosilicon waterproofing agent according to claim 1, characterized in that: The general structural formula of the silane crosslinking agent is R1SiD3; wherein the D group is a hydrolyzable group, and the R group is one or more of a hydrocarbon group and an aromatic group having 3 to 20 carbon atoms.
3. The organosilicon waterproofing agent according to claim 1, characterized in that: The surfactant is a cationic surfactant, an anionic surfactant, a nonionic surfactant or a composite ionic surfactant; wherein the cationic surfactant is selected from one or more of fatty amine salts, ethanolamine salts, and polyethylene polyamine salts to form a cationic emulsion; the anionic surfactant is selected from one or more of anionic polyacrylamide, fatty acid salts, sulfonates, sulfate esters, and phosphate esters to form an anionic emulsion; the nonionic surfactant is selected from one or more of Span series, Tween series, polyethylene glycol fatty acid esters, fatty alcohol polyoxyethylene ethers, alkylphenol polyoxyethylene ethers, isomeric alcohol polyoxyethylene ethers, and nonylphenol polyoxyethylene ethers to form a nonionic emulsion; the composite ionic surfactant is a mixture of a nonionic emulsifier and an ionic emulsifier used as an emulsifier to form a composite ionic emulsion.
4. The organosilicon waterproofing agent according to claim 1, characterized in that: The auxiliary agent is selected from one or more of ethylene glycol, propylene glycol, propylene glycol butyl ether, ethylene glycol butyl ether and a defoaming agent.
5. The organosilicon waterproofing agent according to claim 1, characterized in that: The preservative is selected from one or more of phenoxyethanol, copper nitrate, copper sulfate, dimethylol dimethyl hydantoin, and isothiazolinone.
6. A method for preparing the organosilicon waterproofing agent according to any one of claims 1 to 5, characterized in that: The following steps are involved: a) mixing a silane crosslinking agent, a silane oligomer, a Q-type resin and a surfactant, and then adding water dropwise until a phase inversion is achieved to obtain a crude emulsion; b) The crude emulsion obtained in step a) is homogenized under high pressure, an auxiliary agent and a preservative are added, and the mixture is stirred evenly to obtain an organosilicon waterproofing agent.
7. The preparation method according to claim 6, characterized in that: The mixing process in step a) is carried out in a stirred reactor; the mixing temperature is 10°C to 40°C, the stirring speed is 800r / min to 2000r / min, and the time is 30min to 120min.
8. The preparation method according to claim 6, characterized in that: The pressure of the high-pressure homogenization in step b) is 300 bar to 1200 bar.