Medium-entropy alloy with antibacterial properties, preparation method and application thereof

Through ultrasonic cleaning and smelting and suction casting preparation of (Fe63.3Mn14Si9.1Cr9.8C3.8)88-XCu12AgX medium entropy alloy, the shortcomings of the medium entropy alloy in antibacterial are solved, and high antibacterial performance and excellent without heat treatment are achieved. Mechanical properties, suitable for a variety of high-demand applications.

CN116479341BActive Publication Date: 2024-11-08LANZHOU UNIVERSITY OF TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310433120.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-20
Publication Date
2024-11-08
Estimated Expiration
2043-04-20

AI Technical Summary

Technical Problem

Medium-entropy alloys have very few applications in antibacterial. The mechanical properties of traditional antibacterial alloys such as stainless steel cannot meet the needs of high strength and high toughness, and their antibacterial ability is limited, and it takes more than 12 hours to reach the primary antibacterial level.

Method used

(Fe63.3Mn14Si9.1Cr9.8C3.8)88-XCu12AgX medium-entropy alloy was prepared by ultrasonic cleaning and smelting and suction casting to realize an intermediate-entropy alloy with antibacterial properties without heat treatment.

Benefits of technology

This medium-entropy alloy is better than traditional materials in terms of mechanical properties and antibacterial properties. It can significantly improve the antibacterial effect without heat treatment. It has high yield strength, compressive strength and plastic strain, and has good corrosion resistance and low Permeability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116479341B_ABST
    Figure CN116479341B_ABST
Patent Text Reader

Abstract

The present invention discloses a medium entropy alloy with antibacterial properties, a preparation method and an application thereof. The present invention provides a composition expression of: (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88‑X Cu 12 Ag X , where 1≤x≤5, x is an integer. The alloy can be used in the preparation of components with antibacterial properties, avoiding the problem of traditional materials requiring heat treatment before antibacterial properties; it can also be used in components that require corrosion resistance and a relative magnetic permeability less than 1.04963.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of metal material technology, and in particular to medium-entropy alloys with antibacterial properties, preparation methods, and applications thereof. Medium-entropy alloys are a new type of alloy material with a relatively high entropy value, which lies between that of traditional materials and high-entropy alloys. They have the advantages of high strength, high toughness, and good corrosion resistance, and can be widely used in aviation, navigation, energy, and chemical energy. Currently, medium-entropy alloys are rarely used in antibacterial applications. The most commonly used antibacterial alloy is antibacterial stainless steel, but its mechanical properties cannot meet the requirements of high strength and high toughness, and its antibacterial ability is limited. It takes more than 12 hours to achieve first-level antibacterial properties. Summary of the Invention

[0002] The main purpose of the present invention is to propose a medium-entropy alloy with antibacterial properties, a preparation method and its application, aiming to provide a medium-entropy alloy that can be antibacterial without heat treatment.

[0003] To achieve the above object, the present invention proposes a medium entropy alloy with antibacterial properties, the composition of which is expressed as follows: (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X , where 1≤x≤5 and x is an integer.

[0004] Optionally, x=2.

[0005] A method for preparing a medium-entropy alloy with antibacterial properties is provided, comprising the following steps:

[0006] S1. Weigh the metal components containing Fe, Mn, Si, Cr, C, Cu and Ag, where the atomic proportion of each metal component satisfies the expression (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X The relationship between the various metal components in

[0007] S2, treating the metal components by ultrasonic cleaning to obtain the metal components after ultrasonic cleaning;

[0008] S3. Melting and suction casting the metal components after ultrasonic cleaning to obtain a medium-entropy alloy with antibacterial properties.

[0009] Optionally, in step S3, the metal mixture after ultrasonication is melted using a melting system. After step S2 and before step S3, the melting system is evacuated and filled with argon gas to make the internal vacuum degree of the melting system reach 1×10 -4 Pa.

[0010] Optionally, in step S3, the method of controlling the vacuum degree includes vacuuming and filling with argon.

[0011] Optionally, in step S3, the suction casting includes: using negative pressure suction casting, the mold in the negative pressure suction casting includes a mold composed of two halves spliced ​​together, each halves is cleaned before splicing the mold, and a small amount of silicone grease is evenly applied, and after applying, the two halves of the mold are spliced ​​together, and silicone is used to apply the external gap of the mold and dry it for use.

[0012] Optionally, in step S3, the smelting includes: the smelting crucible for containing the metal components after ultrasonic cleaning is a corundum crucible.

[0013] The present invention provides an application of a medium-entropy alloy with antibacterial properties in preparing a component with antibacterial properties.

[0014] The present invention provides an application of a medium-entropy alloy with antibacterial properties in preparing components with corrosion resistance.

[0015] The present invention provides an application of a medium-entropy alloy with antibacterial properties in preparing a component with a relative magnetic permeability less than 1.04963.

[0016] The technical solution provided by the present invention provides a medium-entropy alloy with antibacterial properties. The mechanical properties and antibacterial properties are superior to those of traditional materials. The antibacterial properties do not require heat treatment, thereby solving the problem that traditional materials need heat treatment before antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying any creative work.

[0018] Figure 1 XRD (X-ray diffraction) detection patterns of medium-entropy alloys under different X-parameters provided in Examples 1 to 5 of the present invention;

[0019] Figure 2 Engineering stress-strain curves of the medium-entropy alloy compression process under different X parameters provided in Examples 1 to 5 of the present invention;

[0020] Figure 3 Figure 2 shows colony culture of the culture medium after 2h, 6h, 12h, and 24h of bacterial coating on the stainless steel 304SS and the medium-entropy alloy provided in Examples 1 to 5 of the present invention and Comparative Example 1, under different X parameters.

[0021] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings and in conjunction with the embodiments. DETAILED DESCRIPTION

[0022] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or the conditions recommended by the manufacturer. Where the reagents or instruments used are not specified by the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes. Taking "A and / or B" as an example, it includes scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical solutions between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in this field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] At present, the application of medium-entropy alloys in antibacterial applications is very rare. The most commonly used antibacterial alloy is stainless steel, but the mechanical properties of stainless steel cannot meet the requirements of high strength and high toughness, and its antibacterial ability is limited. It takes more than 12 hours to reach the first-level antibacterial effect.

[0024] In order to solve the above problems, the present invention provides a medium-entropy alloy with antibacterial properties, a preparation method and application thereof.

[0025] See also Figures 1 to 3 The medium entropy alloy with antibacterial properties has an alloy composition expression of: (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X , where 1≤x≤5, x is an integer, and this application does not make specific restrictions, x can be 1, 2, 3, 4, or 5. Compared with traditional materials, such as stainless steel 304SS, and Fe 63.3 Mn 14 Si9.1 Cr 9.8 C 3.8 The mechanical properties and antibacterial properties of medium entropy alloys are better than those of stainless steel 304SS and Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 , antibacterial properties do not require heat treatment, to solve the problem that traditional materials need heat treatment before antibacterial.

[0026] Specifically, when X=2, (Fe6 3.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 86 Cu 12 Ag2 medium entropy alloy has the best antibacterial and mechanical properties, which can be combined with Figure 2-3 Analyze and get, Figure 2 It can be seen that when X=2, (Fe6 3.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 86 Cu 12 Ag2 has excellent comprehensive properties, with yield strength, compressive strength and plastic strain of 1100.29±1MPa, 1921.56±1MPa and 27.09±0.1% respectively; Figure 3 It can be seen that X=2 has an excellent antibacterial effect.

[0027] The present invention provides a method for preparing a medium-entropy alloy with antibacterial properties, comprising the following steps:

[0028] S1. Weigh the metal components containing Fe, Mn, Si, Cr, C, Cu and Ag, where the atomic proportion of each metal satisfies the expression (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X The relationship between the various metal components in

[0029] S2. Ultrasonic treatment is used to treat the metal components to obtain ultrasonically cleaned metal components. The ultrasonic treatment time is not specifically limited in this application. Generally, the ultrasonic treatment time is preferably about 10 minutes, and the purpose is to remove attachments on the surface of the raw material.

[0030] S3, melting and suction casting the ultrasonicated metal components to obtain a medium-entropy alloy with antibacterial properties;

[0031] After step S2 and before step S3, the placement of each metal component after ultrasonic cleaning is based on the differences in the physical properties of each element, as follows:

[0032] 1. Metal and non-metal elements are matched with each other, that is, C elements are interspersed in metal elements, such as Mn, C, Si, Fe, Cr or Mn, Si, C, Fe, Cr in this order; 2. Elements with lower boiling points should be placed below elements with higher boiling points to prevent them from excessive volatilization, for example: the boiling point of Fe is 2750℃, the boiling point of Mn is 1962℃, the boiling point of Si is 2355℃, the boiling point of Cr is 2761℃, the boiling point of C is 4827℃, the boiling point of Cu is 2595℃, and the boiling point of Ag is 2660℃. The boiling point is 2212℃, that is to say, put in the order of Mn, Si, Cr, and Fe; 3. Cu and Ag are elements that are easy to segregate, so they are put into the corundum crucible together with other elements in a uniform matching method for smelting. For example, when Fe, Mn, Si, Cr, C and other elements are put into the corundum crucible in the order of boiling points, Cu and Ag are randomly interspersed, such as Mn, Cu, Si, Ag, Fe, Cr or Mn, Si, Cu, Fe, Ag, Cr, etc.

[0033] Furthermore, the crucible used for smelting metal in the present application is a corundum crucible, the purpose of which is to keep the temperature after heating, melt the raw materials quickly, and reduce the amount of volatilization.

[0034] Furthermore, in step S3, the metal components after ultrasonic cleaning are melted using a melting system. After step S2 and before step S3, the melting system is evacuated and filled with argon gas to make the internal vacuum degree of the melting system reach 1×10 -4 Pa, vacuum pump and high-purity argon equipment are used respectively to evacuate and fill the melting system with argon. The purpose of evacuating and filling with argon is to prevent metal oxidation.

[0035] In order to achieve the required vacuum degree in the melting system, the specific number of vacuuming and argon filling is not limited, and can be 3 times, 4 times or 5 times, wherein the argon filling has the effect of expelling oxygen and impurities.

[0036] Furthermore, in step S3, the suction casting includes: using negative pressure suction casting, the mold in the negative pressure suction casting includes a mold composed of two halves, each halves are cleaned before the mold is assembled, and a small amount of silicone grease is evenly applied. After applying, the two halves of the mold are assembled together, and silicone is used to smear the external gap of the mold and dry it for use. The present application does not limit the specific material of the mold, and it can be a mold made of a metal that is not easy to react, such as a copper mold, a gold mold, etc.

[0037] Specifically, the suction casting in this application mainly uses a copper mold negative pressure suction casting method. This method uses a copper mold, which is composed of two halves spliced ​​together. The two halves of the copper mold need to be cleaned before use to ensure that the copper mold is smooth and clean. After splicing, silicone is applied to the external gaps of the copper mold to ensure airtightness.

[0038] The present invention provides an application of a medium-entropy alloy with antibacterial properties in preparing a component with antibacterial properties.

[0039] The antibacterial components include all the technical solutions of the medium-entropy alloy, and therefore also have all the beneficial effects brought by the above solutions, which will not be repeated here. The antibacterial components can be used in special equipment including but not limited to hospitals, navigation, aviation, etc.

[0040] The present invention provides an application of a medium-entropy alloy with antibacterial properties in preparing components with corrosion resistance.

[0041] The corrosion-resistant components include all technical solutions of the medium-entropy alloy, and therefore also have all the beneficial effects brought by the above solutions, which will not be repeated here. The corrosion-resistant components can be used in special equipment including but not limited to hospitals, navigation, aviation, etc.

[0042] The present invention provides an application of a medium-entropy alloy with antibacterial properties in preparing a component with a relative magnetic permeability less than 1.04963.

[0043] The components with a relative magnetic permeability of less than 1.04963 include all technical solutions of the medium-entropy alloy and thus have all the beneficial effects brought by the above solutions, which will not be repeated here. The components with a relative magnetic permeability of less than 1.04963 can be used in special equipment including but not limited to hospitals, navigation, aviation, etc.

[0044] The technical solutions of the present invention are further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0045] Example 1

[0046] A medium entropy alloy, whose expression is (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 87 Cu 12 Ag1.

[0047] Example 2

[0048] A medium entropy alloy, whose expression is (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 86 Cu 12 Ag2.

[0049] Example 3

[0050] A medium entropy alloy, whose expression is (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 85 Cu 12 Ag3.

[0051] Example 4

[0052] A medium entropy alloy, whose expression is (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 84 Cu 12 Ag4.

[0053] Example 5

[0054] A medium entropy alloy, whose expression is (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 83 Cu 12 Ag5.

[0055] Comparative Example 1

[0056] One traditional material is stainless steel 304SS.

[0057] Comparative Example 2

[0058] A medium entropy alloy with the structural formula Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 .

[0059] Performance Testing

[0060] 1.1 X-ray diffraction detection

[0061] Phase analysis of the heat-treated and cast alloys was performed using XRD (D8ADVANCE, AXS). The instrument was equipped with a Cu target, emitting Kα rays, operating at a voltage of 40 kV, a current of 40 mA, a scanning range of 30° to 100°, a step size of 0.02°, and a scanning speed of 5° / min.

[0062] 1.2 Compression mechanics testing method

[0063] Before the compression test, the prepared rod specimens were cut at low speed using a specimen cutter according to the national standard GB / T7314-2005, "Metallic Materials Room Temperature Compression Test Method." The compression test was conducted using a universal mechanical testing machine (WDW-100D) for quasi-static room temperature compression.

[0064] 1.3 Antibacterial performance testing

[0065] The sample size for the antibacterial test is a cylindrical specimen with R = 3mm and H = 3mm. The test method uses the film coating method, and then the antibacterial rate is calculated by the plate count method. The specific steps include:

[0066] In the first step, the samples to be tested and all the instruments used in this experiment were sterilized in an autoclave at a temperature of 121°C and kept ready for use.

[0067] The second step is to use a high-precision electronic balance to weigh 0.5g of beef extract, 0.5g of sodium chloride, 1g of peptone, and 1.5g of agar powder. Two 100mL bottles of nutrient solution are prepared in 250mL containers. The nutrient solution is then sterilized to prepare for the subsequent solid culture medium and bacterial solution.

[0068] In the third step, 100 μL of Escherichia coli (or Staphylococcus aureus) was added to the liquid culture medium and cultured in a shaking incubator for 12 hours to obtain an inoculum. 100 μL of the inoculum was then extracted and diluted to 104 times. 100 μL of the bacterial liquid was then extracted and inoculated into the solid culture medium. The culture results were observed after 24 hours to obtain the optimal dilution factor and the original concentration of E. coli.

[0069] Step 4: Dilute the optimal bacterial solution to 0.02 mL / cm 2 The inoculated area was dripped onto the test surface of the sample, covered with sterilized polyethylene film and the edges were folded neatly to prevent the outflow of the bacterial solution, and cultured in a constant temperature box at 35.5℃ for 24 hours;

[0070] Step 5: Take out the sample and use 1mL of eluent to repeatedly clean the polyethylene film and the test surface of the sample. After shaking, dilute the bacterial solution to 10 4CFU / mL, take 1 mL of bacterial solution and inoculate it into solid culture medium to make 3 parallel groups, culture them in a 35.5℃ constant temperature box for 24 hours, observe and count the number of colonies on the culture medium, and calculate the antibacterial rate (%) as follows:

[0071] R(%)=(BA) / B×100%

[0072] Wherein, R is the antibacterial rate, B is the number of viable bacteria in the blank sample (CFU / mL), and A is the number of viable bacteria in the antibacterial sample (CFU / mL).

[0073] 1.4 Corrosion performance test

[0074] Take two test samples and the control group Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 As well as AISI304 alloy, one portion was placed in 3.5% NaCl solution for electrochemical corrosion, and the other portion was placed in Hank's solution for electrochemical corrosion.

[0075] 1.5 Magnetic performance test

[0076] Magnetic detection was performed using a vibrating sample magnetometer (VSM).

[0077] 2. Experimental results

[0078] 2.1 X-ray diffraction test results

[0079] from Figure 1 It can be found that the cast (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X The phase structure of the medium entropy alloy (X = 1, 2, 3, 4, 5%) is composed of FCC1 (matrix phase) and FCC2 (Cu, Ag-rich phase). With the increase of Ag element, the crystal constants of FCC1 phase are and It can be seen that the crystal constant of the matrix FCC1 phase increases with the addition of Ag, which is reflected in the leftward shift of the alloy's main peak in the XRD (X-ray diffraction) spectrum. The main reason for the formation of these two phase structures is that the alloy has a high Cu content. Cu and Ag tend to separate from the matrix and exist in the alloy as the FCC2 second phase.

[0080] 2.2 Results of compression mechanics testing method

[0081] Figure 2 Is cast (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X The engineering stress-strain curves of the medium entropy alloys (X=1, 2, 3, 4, 5%) show that with the change of the Ag content, (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88- X Cu 12 Ag X The yield strength of the medium entropy alloy (X = 1, 2, 3, 4, 5%) shows a trend of first increasing, then decreasing, and finally increasing again. Example 5, i.e. (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 83 Cu 12 Ag5 has the highest yield strength, i.e. 1361.75±3MPa. The compressive strength of the alloy shows a trend of increasing first and then decreasing, among which Example 3, i.e. (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 85 Cu 12 The best compressive strength of Ag3 alloy is 2341.35±3MPa, and the plastic strain of the alloy shows a downward trend. 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 87 Cu 12 The best plastic strain of Ag1 alloy is 28.26±0.2%. However, considering the material cost and the three compression properties, Example 2, i.e. (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 86 Cu 12Ag2 has excellent comprehensive properties, with yield strength, compressive strength and plastic strain being 1100.29±1MPa, 1921.56±1MPa and 27.09±0.1%, respectively.

[0082] 2.3 Antibacterial performance test results

[0083] from Figure 3 As can be seen from Table 1, in the four stages of the interaction between E. coli and the medium entropy alloy film, the number of colonies cultured in the culture medium after 6 hours of interaction with the alloy is very rare, and the presence of colonies is basically invisible on the culture medium after 12 hours and 24 hours of interaction. This also shows that starting from 6 hours, (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X (X = 1, 2, 3, 4, 5%) medium-entropy alloys already have excellent antibacterial effects. However, judging from the results of culture medium alone, it is difficult to see the trend of the alloy's antibacterial effect due to the change in the Ag element, so an additional 2-hour alloy antibacterial test was conducted. As can be seen from the figure, a large number of colonies appeared in the culture medium corresponding to 2 hours compared to other time periods, and as the Ag content increased, the number of colonies on the culture medium increased, and the antibacterial effect showed a downward trend. Among them, the alloy with the least colonies was X = 1, followed by the alloy with X = 2. After six hours, the culture medium with X = 2 had no colonies, and the culture medium with X = 1 had a few colonies.

[0084] Table 1 Antibacterial rate of different alloy samples

[0085]

[0086]

[0087] 2.4 Corrosion performance test results

[0088] As shown in Tables 2 and 3, Example 5 has the best corrosion resistance in a 3.5% NaCl solution. The higher the corrosion potential (Ecorr), the lower the corrosion current density (Icorr), and the larger the R, the better. All of these are better than those in Comparative Example 1, i.e., 304 stainless steel, which also has excellent corrosion resistance in Hank's solution, with a trend similar to that in NaCl solution.

[0089] Table 2 Electrochemical corrosion results of alloys in NaCl solution

[0090]

[0091] Table 3 Electrochemical corrosion results of alloys in Hank's solution

[0092]

[0093]

[0094] 2.5 Magnetic performance test results

[0095] As shown in Table 4, the material is paramagnetic before and after deformation. In other words, its relative magnetic permeability is less than 1.04963 while ensuring strength. It can be used in submarines to avoid detection.

[0096] Table 4 Magnetic permeability of alloy before and after fracture

[0097] Element Relative magnetic permeability before fracture Relative magnetic permeability after fracture Example 1 1.00195 1.02625 Example 2 1.00197 1.02617 Example 3 1.00201 1.02719 Example 4 1.00199 1.02625 Example 5 1.00205 1.02752

[0098] The above description is only a preferred embodiment of the present invention and does not limit the patent scope of the present invention. All equivalent structural transformations made by using the contents of the present invention description and drawings under the inventive concept of the present invention, or direct / indirect application in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A medium entropy alloy with antibacterial properties, characterized in that: The alloy composition is expressed as: (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X , where the subscript is the atomic ratio, 1≤x≤5, and x is an integer.

2. The medium-entropy alloy with antibacterial properties according to claim 1, characterized in that: x=2。 3. The method for preparing a medium-entropy alloy with antibacterial properties according to any one of claims 1 to 2, characterized in that: The following steps are involved: S1. Weigh the metal components containing Fe, Mn, Si, Cr, C, Cu and Ag, where the atomic proportion of each metal component satisfies the expression (Fe 63.3 Mn 14 Si 9.1 Cr 9.8 C 3.8 ) 88-X Cu 12 Ag X The relationship between the various metal components in S2, treating the metal components by ultrasonic cleaning to obtain the metal components after ultrasonic cleaning; S3, melting and suction casting the metal components after ultrasonic cleaning to obtain a medium-entropy alloy with antibacterial properties.

4. The preparation method according to claim 3, characterized in that: In step S3, the metal components after ultrasonic cleaning are melted using a melting system. After step S2 and before step S3, the melting system is evacuated and filled with argon gas to make the internal vacuum degree of the melting system reach 1×10 -4 Pa.

5. The preparation method according to claim 4, characterized in that: In step S3, the method of controlling the vacuum degree includes evacuating the air and filling the air with argon.

6. The preparation method according to claim 5, characterized in that: In step S3, the suction casting includes: using negative pressure suction casting, the mold in the negative pressure suction casting includes a mold composed of two halves spliced ​​together, each halves is cleaned before splicing the mold, a small amount of silicone grease is evenly applied, the two halves of the mold are spliced ​​together after applying, and the external gap of the mold is coated with silicone and dried for use.

7. The preparation method according to claim 6, characterized in that: In step S3, the smelting includes: the smelting crucible used to hold the metal components after ultrasonic cleaning is a corundum crucible.

8. Use of the medium-entropy alloy with antibacterial properties as described in any one of claims 1 to 2 in the preparation of components with antibacterial properties.

9. Use of the medium-entropy alloy with antibacterial properties as described in any one of claims 1 to 2 in the preparation of parts with corrosion resistance.

10. Use of the medium-entropy alloy with antibacterial properties as described in any one of claims 1 to 2 in the preparation of components with a relative magnetic permeability less than 1.04963.

Citation Information

Patent Citations

  • High-plasticity and high-strength zirconium base massive amorphous alloy and preparation method

    CN107287535A

  • Fe-Mn-Cr-Ni-series medium-entropy stainless steel and preparation method thereof

    CN109913769A

  • Antibacterial high-entropy alloy containing copper and silver as well as preparation method and application of antibacterial high-entropy alloy

    CN114606425A

  • Fe-si-la alloy having excellent magneto-caloric properties

    US20110020661A1

  • Metal alloys including copper

    US20170349975A1