Method for making flame retardant blended fabric
By constructing iron hydroxide nanolayers on the surface of flammable blended textiles, the problem of improved flame retardant performance and performance degradation in the prior art is solved, and efficient flame retardant and smoke suppression performance is achieved, while maintaining the skin-friendly and comfortable fabrics. and mechanical strength, and improves water washing resistance.
Patent Information
- Application Number
- CN202310397703.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-13
AI Technical Summary
While improving the flame retardant properties of flammable blended fabrics, existing flame retardant technologies usually reduce their skin-friendly comfort, moisture permeability and mechanical strength, and the interaction force between the flame retardant and the fabric is weak, resulting in It is easy to fall off during use or washing, losing its flame retardant properties.
By soaking the blended fabric in a ferrous ionic salt solution, the oxidation of the active groups on its surface and the ferrous hydroxide nanoparticles are used to form iron hydroxide nanoparticles, and a uniform iron hydroxide nanoflame retardant layer is constructed to improve the flame retardant of the fabric. performance. On the basis of maintaining the original excellent properties of the fabric, this method enhances its flame retardant and smoke suppression properties, and improves water washing resistance by tightly wrapping the fiber gap.
The flame retardant performance improvement is achieved without reducing the skin-friendliness and permeability of the fabric, while improving the mechanical properties of the fabric, and enhancing its washing resistance and flame retardant performance through a stable iron hydroxide nanolayer.
Smart Images

Figure CN116479645B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of textile preparation, and particularly relates to a method for preparing a flame-retardant blended fabric. Background Art
[0002] Blended fabrics such as wool / nylon blended fabric (W / N) and polyester / cotton blended fabric are widely used due to their comfortable skin-friendliness, water permeability and good mechanical properties. However, some blended fabrics are extremely easy to burn due to the introduction of flammable materials. Taking wool / nylon blended fabric as an example, nylon is a polymer compound with a high content of hydrocarbon chain breaks. It is very easy to ignite in the air, and it produces a large amount of molten droplets and releases toxic smoke when burning. When nylon is blended with wool, it will produce a "wick effect" when it burns, and the combustion is more intense, causing greater fire hazards. Therefore, improving the flame retardant properties of flammable blended fabrics is of great practical significance.
[0003] In blended fabrics, wool and other surfaces contain a large number of active groups (-COOH, -OH, -NH 2 ), is an amphoteric polyelectrolyte that can form covalent bonds with phosphorus and coordination bonds with metal ions. Therefore, phosphorus-based flame retardants or metal compounds are often used to treat W / N with halogen-free flame retardancy to achieve condensed phase flame retardancy. For example, Yang Xuhong et al. loaded organic phytic acid and polyethyleneimine compounds on W / N by deposition to construct an expansion flame retardant system, which effectively improved the flame retardant properties of W / N [Cheng XW, Tang RC, Yao F, et al. Flame retardant coating of wool fabric withphytic acid / polyethyleneimine polyelectrolyte complex[J]. Progress in Organic Coatings, 2019, 132: 336-342.]. Koparal et al. used compounds containing metal zirconium or titanium to react with W / N to achieve flame retardant modification by forming coordination bonds. Metal zirconium or titanium can catalyze the rapid carbonization of nylon / wool blended fabrics during combustion to form a protective layer [Kaynak E, ME, Koparal AS. Halogen free flame retardant finishing of wool and wool rich fabrics for aircraft seats [J]. Materials Today: Proceedings, 2020, 31: S258-S262]. However, the above flame retardant methods all ignore the non-toxicity, skin-friendly comfort and water permeability of the blended fabric itself, and reduce its mechanical strength, affecting its performance. In addition, due to the weak interaction between the flame retardant and the blended fabric, it is easy to fall off during use or washing, thereby losing its flame retardant properties.
[0004] Therefore, how to design environmentally friendly and non-toxic flame retardant technology to improve the flame retardant properties, smoke suppression properties, and better water washability of blended fabrics while maintaining their excellent skin-friendly comfort, water permeability, and high mechanical strength is one of the problems that need to be solved urgently in the current flame retardant field. Summary of the invention
[0005] The present invention aims to provide a method for producing a flame-retardant blended fabric, which improves the flame-retardant properties of a flammable blended fabric while ensuring the skin-friendly comfort, water-permeability and high mechanical strength of the blended fabric itself.
[0006] A method for making a flame retardant blended fabric in this scheme comprises the following steps:
[0007] Step 1: Soak the blended fabric in a ferrous ion salt solution. The surface of the blended fabric contains -COOH, -OH and -NH 2 At least one of the groups;
[0008] Step 2: placing the soaked blended fabric in a constant temperature water bath for 15 to 35 hours, then taking it out and drying it to obtain the flame retardant blended fabric.
[0009] Beneficial effects of this solution: The present invention utilizes -COOH, -OH and -NH 2Taking advantage of the strong coordination effect between groups and metal ions and the difference in stability between ferrous hydroxide and ferric hydroxide, ferrous salt is used as a precursor, which is first hydrolyzed to generate ferrous hydroxide particles, and then gradually converted into more stable ferric hydroxide nanoparticles under the slow oxidation of oxygen in the air, thereby constructing a uniform ferric hydroxide nano-flame retardant layer on the surface of the blended fabric to obtain a blended fabric with excellent flame retardant properties. The preparation process is simple and can be applied on a large scale; in addition, the prepared flame-retardant blended fabric not only has excellent flame retardant and smoke suppression properties, but also has certain improvements in its mechanical properties. At the same time, because the ferric hydroxide nano-flame retardant layer constructed on the surface of the blended fabric tightly wraps the fabric fibers and fills less of the gaps between the fibers of the blended fabric, it almost maintains the skin-friendly comfort and water permeability of the blended fabric itself.
[0010] Furthermore, the blended fabric is wool / nylon blended fabric (W / N), polyester / cotton blended fabric, nylon / cotton blended fabric or nylon / silk blended fabric.
[0011] Furthermore, the ferrous ion salt solution is ferrous sulfate (FeSO 4 ), ferrous chloride (FeCl 2 ) and ferrous nitrate (Fe(NO 3 ) 2 ) at least one of.
[0012] Furthermore, in step 1, the concentration of ferrous ions in the ferrous ion salt solution is 0.1-1.5 mol / L.
[0013] Furthermore, in step 1, after the blended fabric is immersed in the ferrous ion salt solution, the blended fabric is completely soaked in the ferrous ion salt solution by stirring or shaking.
[0014] Furthermore, in step 2, the temperature of the constant temperature water bath is 25-40° C. This temperature range can better control the growth kinetics of the iron hydroxide nanoparticles.
[0015] Furthermore, in step 2, the drying temperature is 25-90° C. This temperature range helps prevent the iron hydroxide nanoparticles from agglomerating.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] (1) The in-situ growth of iron hydroxide nanoparticles on the surface of flammable blended fabrics is carried out by oxidation induction, which can simply and effectively control the growth kinetics of iron hydroxide nanoparticles and produce iron hydroxide nanoparticles with uniform distribution and small particle size.
[0018] (2) Make full use of the -COOH, -OH and -NH 2The strong coordination effect of active groups with ferrous ions and ferric ions effectively improves the bonding strength between the nano flame retardant and the substrate, thereby obtaining better water washability.
[0019] (3) As an efficient and environmentally friendly flame retardant, ferric hydroxide has cheap raw materials and low production cost; the preparation process is simple and easy to achieve mass production;
[0020] (4) While improving the flame retardant and smoke suppression properties of W / N, the original excellent mechanical properties of W / N are maintained. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a surface SEM photo of the flame retardant W / N prepared in Example 1;
[0022] Figure 2 This is a photo of the flame retardant W / N prepared in Example 1 after vertical combustion performance test;
[0023] Figure 3 Cone calorimetry HRR curves of flame retardant W / N and conventional W / N prepared in Example 1;
[0024] Figure 4 Cone calorimetry THR curves of flame retardant W / N and conventional W / N prepared in Example 1;
[0025] Figure 5 Cone calorimetry SPR curves of flame retardant W / N and conventional W / N prepared in Example 1;
[0026] Figure 6 Cone calorimetry TSP curves of flame retardant W / N and conventional W / N prepared in Example 1;
[0027] Figure 7 This is the surface SEM photo of the flame-retardant W / N prepared in Example 1 after being washed with water for 24 hours. DETAILED DESCRIPTION
[0028] The following is further described in detail through specific implementation methods:
[0029] The present invention is described in detail below through examples, and the technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.
[0030] It is necessary to point out that this embodiment is only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by technicians in this field based on the above invention content are also considered to fall within the scope of protection of the present invention. It should be emphasized that the substrate size in the specific embodiment described here is only used to describe the content of the present invention in detail and is not used to limit the present invention.
[0031] The present invention provides a method for producing a flame retardant blended fabric, the process steps and conditions of the method are as follows (the parts of materials used in the following examples are all parts by weight unless otherwise specified):
[0032] Example 1
[0033] A method for producing a flame retardant blended fabric comprises the following steps:
[0034] First, 30 × 10 cm W / N was immersed in 1500 mL 0.1 mol / L ferrous sulfate solution and shaken for 5 min;
[0035] Then, the fully soaked W / N was placed in a constant temperature water bath and maintained at 30°C for 24 hours; finally, the W / N was taken out and dried in an oven at 90°C for 2 hours to obtain the flame retardant W / N.
[0036] Performance Test:
[0037] (1) Surface morphology test
[0038] The surface morphology of the W / N fabrics was observed using a JEOL JSM-5900LV scanning electron microscope (SEM), and the surface of the samples was sprayed with gold before testing.
[0039] The test shows that after the flame retardant treatment, a large amount of Fe(OH) is evenly attached to the surface of the W / N fabric. 3 Nanoparticles, the particle size of which is about 110nm, are Figure 1 shown.
[0040] (2) Limiting oxygen index (LOI) test
[0041] The limiting oxygen index test is a common test method for modern flame retardant materials. It refers to the minimum oxygen concentration required for the tested material to burn smoothly in a nitrogen-oxygen mixture. This patent uses the JF-3 oxygen index tester for testing in accordance with GB / T 5454-1997. The sample size is 125mm×20mm. Each group of samples is tested three times on average. The final result is the average value. The test result evaluation criteria are shown in Table 1.
[0042] Table 1 Limiting oxygen index rating table
[0043]
[0044] It has been determined that the LOI of the flame retardant W / N can be as high as 31.6%, reaching the level of flame retardant materials.
[0045] (3) Vertical burning level test
[0046] This patent uses a CZF-3 vertical combustion apparatus to test the flame retardant properties of samples in accordance with the UL-94 test standard. The sample size is 275mm×75mm. The specific judgment criteria are shown in Table 2.
[0047] Table 2 Vertical burning test requirements
[0048]
[0049] The flame retardant W / N has passed the UL-94 test V-0 grade. Figure 2 shown.
[0050] (4) Cone Calorimeter (CC) test
[0051] CC is a combustion behavior research instrument designed based on the principle of oxygen consumption. It characterizes the combustion behavior of materials by measuring combustion parameters such as time to ignition (TTI), heat release rate (HRR), total heat release (THR), smoke product rate (SPR), and total smoke production (TSP). It is currently recognized as the most ideal small combustion performance test instrument. The CC test of the sample in this patent was conducted using the cone calorimeter of Kunshan Modisco Combustion Technology Instrument Co., Ltd., with an irradiation power of 35kW / m 2 , the sample size is 100mm×100mm.
[0052] After testing, the HRR peak of the flame retardant W / N was reduced to 185.6kW m -2 , as attached Figure 3 As shown; the THR value is reduced to 6.16MJ m -2 , as attached Figure 4 As shown in the figure, compared with the unflame-retardant W / N, the SPR peak and TSP values of the flame-retardant W / N were reduced by 48.5% and 15.0%, respectively. In addition, the SPR peak and TSP values of the flame-retardant W / N were reduced to 0.006m 2 s -1 and 0.09m 2 , as shown in the attached Figure 5 and attached Figure 6 As shown; compared with W / N without flame retardant treatment, it was reduced by 76.92% and 55.0% respectively.
[0053] (5) Washability test
[0054] The flame retardant W / N was immersed in 600 mL of water, magnetically stirred for 24 h, and then taken out and dried to observe the Fe(OH) 3 Changes in nanoparticles.
[0055] After testing, a large amount of Fe(OH) was still attached to the surface of the flame retardant W / N after 24 hours of water washing. 3 Nanoparticles (such as Figure 7 As shown), and it still exhibits excellent flame retardant properties, indicating that the prepared flame retardant W / N has good water washability.
[0056] The above test results show that the flame retardant treatment greatly improves the flame retardant and smoke suppression properties of W / N fabrics, and the flame retardant W / N has excellent water washability.
[0057] Example 2
[0058] A method for producing a flame retardant blended fabric comprises the following steps:
[0059] First, 30 × 10 cm W / N was immersed in 1500 mL 0.8 mol / L ferrous sulfate solution and shaken for 5 min;
[0060] Then, the fully soaked W / N was placed in a constant temperature water bath and maintained at 30°C for 24 hours; finally, the W / N was taken out and dried in an oven at 90°C for 2 hours to obtain the flame retardant W / N.
[0061] SEM observation of the flame retardant W / N surface showed that a large amount of Fe(OH) 3 The flame retardant W / N has a LOI value of 30.0%, passes the UL-94 test V-0 level, and its HRR peak value is reduced from 360.1 to 221.5kW / m 2 , THR decreased from 7.25 to 6.25 MJ / m 2 , the SPR peak value decreased from 0.026 to 0.009m 2 / s, TSP value decreased from 0.20 to 0.11m 2 .
[0062] Example 3
[0063] A method for producing a flame retardant blended fabric comprises the following steps:
[0064] First, 30 × 10 cm W / N was immersed in 1500 mL 0.6 mol / L ferrous chloride solution and shaken for 5 min;
[0065] Then, the fully soaked W / N was placed in a constant temperature water bath at 25°C for 24 h;
[0066] Finally, the W / N was taken out and dried in an oven at 90°C for 2 h to obtain the flame retardant W / N.
[0067] SEM observation of the flame retardant W / N surface showed that a large amount of Fe(OH) 3 The flame retardant W / N produced by the test has a LOI value of 32.1%, passes the UL-94 test V-0 level, and its HRR peak value is reduced from 360.1 to 242.9kW / m 2 , THR decreased from 7.25 to 6.31 MJ / m 2 , the SPR peak value decreased from 0.026 to 0.008m 2 / s, TSP value decreased from 0.20 to 0.10m 2 .
[0068] Example 4
[0069] A method for making a flame retardant blended fabric comprises the following steps:
[0070] First, 30 × 10 cm W / N was immersed in 1500 mL 0.4 mol / L ferrous sulfate solution and shaken for 5 min;
[0071] Then, the fully soaked W / N was placed in a constant temperature water bath at 40°C for 24 h;
[0072] Finally, the W / N was taken out and dried in an oven at 70°C for 2 h to obtain the flame retardant W / N.
[0073] SEM observation of the flame retardant W / N surface showed that a large amount of Fe(OH) 3 The flame retardant W / N produced by the test has a LOI value of 28.4%, passes the UL-94 test V-0 level, and its HRR peak value is reduced from 360.1 to 246.2kW / m 2 , THR decreased from 7.25 to 6.36 MJ / m 2 , the SPR peak value decreased from 0.026 to 0.011m 2 / s, TSP value decreased from 0.20 to 0.12m 2 .
[0074] Example 5
[0075] A method for making a flame retardant blended fabric comprises the following steps:
[0076] First, 30 × 10 cm W / N was immersed in 1500 mL 0.6 mol / L ferrous sulfate solution and shaken for 5 min;
[0077] Then, the fully soaked W / N was placed in a constant temperature water bath and maintained at 30°C for 24 hours; finally, the W / N was taken out and dried in an oven at 40°C for 6 hours to obtain the flame retardant W / N.
[0078] SEM observation of the flame retardant W / N surface showed that a large amount of Fe(OH) 3 The flame retardant W / N produced by the test has a LOI value of 28.9%, passes the UL-94 test V-0 level, and its HRR peak value is reduced from 360.1 to 252.8kW / m 2 , THR decreased from 7.25 to 6.43 MJ / m 2 , SPR peak value decreased from 0.026 to 0.013m 2 / s, TSP value decreased from 0.20 to 0.14m 2 .
[0079] The performance testing method of the flame retardant W / N prepared in Examples 2 to 5 is the same as that in Example 1, and will not be repeated here.
Claims
1. A method for producing a flame retardant blended fabric, characterized in that: The following steps are involved: Step 1, immersing the blended fabric in a ferrous ion salt solution, wherein the surface of the blended fabric contains at least one of -COOH, -OH and -NH2 groups; Step 2, placing the soaked blended fabric in a constant temperature water bath for 15 to 35 hours, and then taking it out to dry, thereby obtaining the flame retardant blended fabric; In step 1, the concentration of ferrous ions in the ferrous ion salt solution is 0.1-1.5 mol / L; in step 2, the temperature of the constant temperature water bath is 25-40° C., and the drying temperature is 25-90° C.; Using ferrous salt as a precursor, it is first hydrolyzed to form ferrous hydroxide particles, and then gradually converted into more stable ferric hydroxide nanoparticles under the slow oxidation effect of oxygen in the air, thereby constructing a uniform ferric hydroxide nano-flame retardant layer on the surface of the blended fabric.
2. The method for producing a flame retardant blended fabric according to claim 1, characterized in that: The blended fabric is wool / nylon blended fabric, polyester / cotton blended fabric, nylon / cotton blended fabric or nylon / silk blended fabric.
3. The method for producing a flame retardant blended fabric according to claim 2, characterized in that: The ferrous ion salt solution is at least one of ferrous sulfate, ferrous chloride and ferrous nitrate.
4. The method for producing a flame retardant blended fabric according to any one of claims 1 to 3, characterized in that: In step 1, after the blended fabric is immersed in the ferrous ion salt solution, the ferrous ion salt solution is stirred or shaken to completely soak the blended fabric.