NO adsorbent and preparation method and application thereof
The MgCo2O4-BaCO3/AC adsorbent was prepared by co-precipitation method and combined with microwave catalysis method, which solved the problems of low adsorption capacity and high operating cost of the adsorbent, achieved efficient NO adsorption and decomposition, reduced operating costs, and improved NO conversion. Rate.
Patent Information
- Application Number
- CN202310575908.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-05-22
AI Technical Summary
In the existing nitrogen oxide removal technology, the adsorbent has low adsorption capacity, high operating cost, and the catalyst operating temperature range is narrow, making it difficult to efficiently treat large flow and low concentration NO flue gas.
MgCo2O4-BaCO3/AC adsorbent was prepared by co-precipitation method. MgCo2O4 and BaCO3 were loaded on the surface of activated carbon particles to form spinel structure and rod-like structure, which synergistically increased the adsorption capacity, and combined with microwave catalytic method to alternately treat NO.
It achieves efficient adsorption and decomposition of NO, with an adsorption capacity of 40.2 mg/g, reducing operating costs, and the system operates reliably, with a NO conversion rate of up to 99.7%.
Smart Images

Figure CN116492987B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of nitrogen oxide removal, and specifically relates to a NO adsorbent and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides are one of the main pollutants that seriously endanger human health. More than 95% of them are NO. It can be seen that controlling NO emissions is extremely important.
[0003] At present, the technologies for removing nitrogen oxides mainly include selective catalytic reduction (SCR), selective non-catalytic reduction (SNCR), catalytic direct decomposition, pulse corona, electron beam denitrification technology, liquid absorption, solid adsorption and microbial treatment. Among them, the technology with the highest removal efficiency and the most mature, which has been widely used in industry, is the selective catalytic reduction technology (NH3-SCR) with NH3 as the reducing agent, but this technology has obvious disadvantages: ① The ammonia consumption is too large, and the stoichiometric ratio of NH3 must be strictly controlled, otherwise the unreacted NH3 will cause secondary pollution; ② NH3 is a toxic and corrosive gas, which is dangerous in storage and transportation, has high requirements for pipeline equipment and is expensive; ③ NH3 reacts with SO2 in flue gas to form corrosive NH4HSO4, which can easily poison the catalyst. ④ The current operating temperature range of the catalyst is narrow (623K~673K). Several other technologies also have technical problems. For example, the liquid absorption method has low denitrification efficiency and poor purification effect; the solid adsorption method has a small adsorption capacity and frequent regeneration; the microbial method is in the experimental stage, and the empty tower gas velocity of the packed tower, flue gas temperature, cultivation of denitrifying bacteria, bacterial growth rate and packing clogging are all issues that need to be resolved; how to achieve high power, narrow pulse and long life of the high-voltage pulse power supply in the pulse corona method needs to be resolved; the electron beam denitrification technology has high energy consumption.
[0004] The inventor disclosed a composite catalyst for microwave catalysis and a method for catalytically decomposing NO in the prior patent document CN201810101669.8. The MgCo2O4-BaCO3 composite catalyst provided in the application can directly catalytically decompose NO into N2 and O2. Although the use of the MgCo2O4-BaCO3 composite catalyst for microwave heating denitration of NO can achieve a higher conversion rate, when this method is used to treat NO in a large flow and low concentration state, there is still a problem of high energy consumption caused by continuous microwave output.
[0005] The inventor disclosed a denitrification method for directly decomposing NO by adsorption-microwave catalysis in the prior patent document CN202211148627.2. In this application, the adsorbent and the catalyst are mixed and filled into the reaction tube of the reactor to form an adsorption-microwave catalytic reaction bed. The adsorption treatment and microwave catalysis treatment are alternately performed to first adsorb NO and then decompose NO to achieve the purpose of denitrification. However, this method still has the problems of frequent operation and high operating cost due to insufficient adsorption capacity of the adsorbent. Summary of the invention
[0006] The purpose of the present invention is to improve a NO adsorbent expressed as MgCo2O4-BaCO3 / AC, which has a high adsorption capacity, solves the technical problem of low adsorption capacity of adsorbents in the prior art, and is applied to the treatment of flue gas containing NO, with the advantages of higher efficiency and more energy saving.
[0007] In order to achieve the above object, the present invention provides a NO adsorbent, wherein the NO adsorbent is expressed as MgCo2O4-BaCO3 / AC, wherein the MgCo2O4-BaCO3 / AC adsorbent is obtained by loading MgCo2O4 and BaCO3 on the surface of activated carbon particles by a coprecipitation method, wherein the MgCo2O4 is rich in NO x The spinel structure of the adsorption site, the BaCO3 is a rod-shaped structure, and the synergistic effect of the MgCo2O4, the BaCO3 and the activated carbon makes the NO adsorbent have a high adsorption capacity, wherein the mass ratio of the MgCo2O4-BaCO3:AC is (0.1-0.4):1, and the mass ratio of MgCo2O4:BaCO3 in the MgCo2O4-BaCO3 is 1:(0.1-0.6).
[0008] Preferably, the mass ratio of the MgCo2O4-BaCO3:AC is (0.1-0.2):1, and the mass ratio of MgCo2O4:BaCO3 in the MgCo2O4-BaCO3 is 1:(0.4-0.6).
[0009] More preferably, the mass ratio of the MgCo2O4-BaCO3:AC is 0.2:1, and the mass ratio of MgCo2O4:BaCO3 in the MgCo2O4-BaCO3 is 1:0.5.
[0010] Preferably, the adsorption capacity of the NO adsorbent is 16 to 40.2 mg / g.
[0011] In a specific embodiment, the MgCo2O4-BaCO3 / AC adsorbent is prepared by the following method, comprising the following steps:
[0012] Step 1, dispersing the pretreated activated carbon particles in deionized water to obtain a dispersion;
[0013] Preferably, the pretreatment step of the activated carbon particles comprises: dispersing the activated carbon in a KOH solution, stirring at 70-90° C. for 1.5-3 h, filtering after cooling, washing with deionized water until neutral, drying at 100-120° C., and grinding through an 80-mesh sieve to obtain the activated carbon particles.
[0014] Step 2: Add Mg(NO3)2 solution, Co(NO3)2 solution and Ba(NO3)2 solution to the dispersion according to a preset mass ratio, stir evenly, then add carbonate solution drop by drop, stir at 40-50°C for 1.5-3h, obtain a precipitate by solid-liquid separation, wash, dry, grind, sieve and calcine the precipitate to obtain the catalyst to be treated;
[0015] Preferably, the carbonate is one of potassium carbonate and sodium carbonate, or a mixture of the two.
[0016] Preferably, the solid-liquid separation method is centrifugal separation.
[0017] Preferably, the drying temperature is 100-120° C., and the drying time is 14-18 hours.
[0018] Preferably, the calcination conditions include: a calcination temperature of 200-350° C. and a calcination time of 1 to 2 hours.
[0019] Step 3: placing the catalyst to be treated in a microwave reactor and treating it for 15 to 30 minutes under the first preset microwave conditions to obtain a MgCo2O4-BaCO3 / AC adsorbent.
[0020] Preferably, the first preset microwave conditions include: oxygen-free conditions, a microwave heating temperature of 200-400° C., and a microwave frequency of 600-2350 MHz for microwave heating treatment.
[0021] More preferably, the oxygen-free condition is to introduce any one of nitrogen, argon and helium as a protective gas.
[0022] The present invention also provides a method for preparing a NO adsorbent, the method comprising the following steps:
[0023] (1) dispersing the pretreated activated carbon particles in deionized water to obtain a dispersion;
[0024] (2) adding Mg(NO3)2, Co(NO3)2, and Ba(NO3)2 to the dispersion in a preset mass ratio, stirring evenly, and then adding a carbonate solution dropwise, stirring at 40-50°C for 1.5-3h, and obtaining a precipitate by solid-liquid separation. The precipitate is washed, dried, ground, sieved, and calcined to obtain a catalyst to be treated;
[0025] (3) placing the catalyst to be treated in a microwave reactor and treating it under the first preset microwave conditions for 15 to 30 minutes to obtain a MgCo2O4-BaCO3 / AC adsorbent, wherein the mass ratio of the MgCo2O4-BaCO3:AC is (0.1-0.4):1, and the mass ratio of MgCo2O4:BaCO3 in the MgCo2O4-BaCO3 is 1:(0.1-0.6).
[0026] In a specific embodiment, the first preset microwave conditions in step (3) include: oxygen-free conditions, a microwave heating temperature of 200-400° C., and a microwave frequency of 500-3000 MHz for microwave heating treatment.
[0027] In a specific embodiment, the anaerobic condition is to introduce any one of nitrogen, argon and helium as a protective gas.
[0028] In a specific embodiment, the carbonate in step (2) is one of potassium carbonate and sodium carbonate, or a mixture of the two.
[0029] Preferably, the concentration of the carbonate is 0.2 mol / L.
[0030] In a specific embodiment, in step (2), the drying conditions include: a drying temperature of 100 to 120° C. and a drying time of 12 to 18 hours.
[0031] In a specific embodiment, the calcination conditions in step (2) include: a calcination temperature of 200-350° C., and a calcination time of 1 to 2 hours.
[0032] It should be noted that the Mg(NO3)2 added in step (2) can be a prepared Mg(NO3)2 solution or Mg(NO3)2·6H2O; the Co(NO3)2 added in step (2) can be a prepared Co(NO3)2 solution or Co(NO3)2·6H2O; the Ba(NO3)2 added in step (2) can be a prepared Ba(NO3)2 solution or Ba(NO3)2 solid.
[0033] In a specific embodiment, the pretreatment step of the activated carbon particles in step (1) includes: dispersing the activated carbon in a KOH solution, stirring at 70-90° C. for 1.5-3 h, filtering after cooling, washing with deionized water until neutral, drying at 100-120° C., and grinding through an 80-mesh sieve to obtain activated carbon particles.
[0034] Wherein, the concentration of the KOH solution is 1 mol / L.
[0035] The present invention also provides a NO adsorbent, which is prepared by the preparation method described above.
[0036] The present invention also provides a use of the NO adsorbent described above in treating waste gas or flue gas containing NO.
[0037] The present invention also provides a method for treating flue gas containing NO, comprising the following steps:
[0038] Filling a NO adsorbent and a microwave catalyst at different positions in a reaction tube of a reactor respectively to form an adsorption-microwave catalytic reaction bed, wherein the NO adsorbent is the NO adsorbent described above;
[0039] At least one alternating treatment is adopted to remove NO in the sintering flue gas, wherein each alternating treatment comprises: passing the sintering flue gas to be treated into the adsorption-microwave catalytic reaction bed, adsorbing NO by the NO adsorbent, and after a preset adsorption time, switching the gas passing into the adsorption-microwave catalytic reaction bed to N2, and under a second preset microwave condition, under the catalytic action of the NO adsorbent and the microwave catalyst, decomposing the NO adsorbed by the NO adsorbent into N2 and O2.
[0040] In a specific embodiment, the microwave catalyst is a MgCo2O4-BaCO3 composite catalyst or a BaMn 0.9 Mg 0.1 O3 catalyst, the second preset microwave conditions include: microwave heating temperature is 100-400°C, and microwave frequency of microwave heating treatment is 500-3000MHz.
[0041] In a specific embodiment, the microwave heating temperature is 200-300° C., and the microwave frequency of the microwave heating treatment is 500-2350 MHz.
[0042] In a specific embodiment, the microwave frequency of the microwave heating treatment is 856-965 MHz.
[0043] In a specific embodiment, when the flue gas is subjected to microwave catalytic decomposition in the adsorption-microwave catalytic reaction bed, the residence time is 0.5s to 10s, preferably 1 to 3s.
[0044] In a specific embodiment, the conditions of the adsorption treatment include: not turning on the microwave and the adsorption temperature is room temperature.
[0045] In a specific embodiment, the preset adsorption time is 10 to 13 hours.
[0046] In a specific embodiment, when the flue gas is subjected to adsorption treatment in the adsorption-microwave catalytic reaction bed, the residence time is 0.5s to 10s, preferably 1 to 3s.
[0047] The beneficial effects of the present invention include at least:
[0048] 1. The present invention provides a NO adsorbent, the expression of the adsorbent is MgCo2O4-BaCO3 / AC, the MgCo2O4-BaCO3 / AC adsorbent is obtained by loading MgCo2O4 and BaCO3 on the surface of activated carbon particles by co-precipitation method, the MgCo2O4 is rich in NO x The spinel structure of the adsorption site, the BaCO3 is a rod-shaped structure, the adsorbent has a high adsorption capacity, the maximum adsorption capacity reaches 40.2 mg / g, and the longest adsorption time can reach 13 hours. In this way, when the adsorption-microwave catalytic method is used to treat NO in flue gas or exhaust gas, frequent operation is not required, the operating cost can be greatly reduced, and the system can operate reliably for a long time.
[0049] 2. Based on the experimental data, the 20% MgCo2O4-0.5BaCO3 / AC adsorbent provided by the present invention has a higher NO adsorption capacity than the AC adsorbent, 20% MgCo2O4 / AC adsorbent, and 20% BaCO3 / AC adsorbent, indicating that MgCo2O4, BaCO3 and activated carbon work synergistically to give the NO adsorbent a high adsorption capacity.
[0050] 3. The method for treating flue gas containing NO provided by the present invention adopts at least one alternating treatment to remove NO from the flue gas, wherein each alternating treatment comprises: passing the flue gas to be treated into the adsorption-microwave catalytic reaction bed, adsorbing NO through the NO adsorbent, switching the gas passing into the adsorption-microwave catalytic reaction bed to N2 after a preset adsorption time, and decomposing the NO adsorbed by the NO adsorbent into N2 and O2 under the catalytic action of the NO adsorbent and the microwave catalyst under a second preset microwave condition; when the preset adsorption time can reach 13h, at a reaction temperature of 250°C, under superoxic conditions (the oxygen content in the flue gas or waste gas is as high as 10%), the NO conversion rate is as high as 99.7%. NO is first adsorbed, and then desorbed after being adsorbed, and then decomposed to generate environmentally friendly N2 and O2. The method has the advantages of simple process, low operating temperature, oxidation resistance, energy saving, high removal efficiency, low operating cost, long-term reliable system operation and no secondary pollution. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is a scanning electron microscope image of the 20% MgCo2O4-0.5BaCO3 / AC adsorbent prepared in Example 1;
[0052] Figure 2 The X-ray diffraction (XRD) spectrum of the 20% MgCo2O4-0.5BaCO3 / AC adsorbent prepared in Example 1;
[0053] Figure 3 Schematic diagram of the removal of NO by the adsorption-microwave catalytic method using the 20% MgCO2O4-0.5BaCO3 / AC adsorbent and the MgCO2O4-40% BaCO3 catalyst prepared in Example 1;
[0054] Figure 4 X-ray photoelectron spectroscopy (XPS, O 1s) graphs of the 20% MgCO2O4 / AC adsorbent prepared in Example 1, the 20% MgCO2O4-0.5BaCO3 / AC adsorbent prepared in Comparative Example 2, and the 20% BaCO3 / AC adsorbent prepared in Comparative Example 3;
[0055] Figure 5 Schematic diagram of the adsorbents prepared in Comparative Examples 1 to 3 respectively combined with MgCO2O4-40%BaCO3 catalysts to remove NO by adsorption-microwave catalysis;
[0056] Figure 6 Schematic diagram of the adsorption capacity of the NaY-MgCo2O4-40%BaCO3 adsorbent in Comparative Example 4 and the 20%MgCO2O4-0.5BaCO3 / AC adsorbent prepared in Example 1;
[0057] Figure 7 Schematic diagram of the removal of NO by adsorption-microwave catalysis corresponding to Comparative Example 5;
[0058] Figure 8 The NO adsorption capacity and NO conversion rate of the adsorbents prepared in Examples 2 to 5 were respectively combined with MgCO2O4-40%BaCO3 catalysts to remove NO using an adsorption-microwave catalytic method;
[0059] Fig. 9 The NO adsorption capacity and NO conversion rate of the adsorbents prepared in Example 1, Example 3, Example 6 and Example 7 were respectively combined with the MgCO2O4-40%BaCO3 catalyst to remove NO using the adsorption-microwave catalytic method;
[0060] Fig.10 The 20% MgCO2O4-0.5BaCO3 / AC adsorbent prepared in Example 1 and the MgCO2O4-40% BaCO3 catalyst, and the 20% MgCO2O4-0.5BaCO3 / AC adsorbent prepared in Example 1 and the BaMn 0.9 Mg 0.1 Schematic diagram of the removal of NO by O3 catalyst using adsorption-microwave catalysis. DETAILED DESCRIPTION
[0061] The present invention is described in detail below with reference to the accompanying drawings and embodiments, but the present invention can be implemented in many different ways as limited and covered by the claims.
[0062] It should be noted that, in the following text, x% in x%MgCo2O4-yBaCO3 / AC adsorbent means that the mass content of MgCo2O4-BaCO3 in the x%MgCo2O4-yBaCO3 / AC adsorbent is x%, and y means that the mass of BaCO3 in the MgCo2O4-BaCO3 is y times the mass of MgCo2O4.
[0063] Example 1
[0064] 1. Preparation of adsorbent:
[0065] A 20% MgCo2O4-0.5BaCO3 / AC adsorbent was prepared, wherein the mass content of MgCo2O4-BaCO3 in the 20% MgCo2O4-0.5BaCO3 / AC adsorbent was 20%, and the mass of BaCO3 in the MgCo2O4-BaCO3 was 0.5 times the mass of MgCo2O4.
[0066] To prepare the adsorbent, the amount of activated carbon particles added was 2.5 g, the amount of Mg(NO3)2·6H2O added was 0.52 g, the amount of Co(NO3)2·6H2O added was 1.18 g, and the amount of Ba(NO3)2 added was 0.35 g.
[0067] Step 1.1, carrier pretreatment: disperse activated carbon (AC) in KOH solution (the concentration of KOH solution is 1 mol / L), stir at 70-90°C for 1.5-3h, filter after cooling, wash with deionized water until neutral, dry at 100-120°C, grind through 80 mesh sieve, and prepare activated carbon particles with a particle size of 80 mesh.
[0068] Step 1.2, prepare the adsorbent by co-precipitation method: weigh activated carbon particles and disperse them in deionized water to obtain a dispersion, weigh Mg(NO3)2·6H2O, Co(NO3)2·6H2O, and Ba(NO3)2 according to a preset mass ratio and dissolve them in the dispersion, stir for 30 minutes, then drop by drop an aqueous solution dissolved with potassium carbonate (the concentration of the potassium carbonate solution is 0.2 mol / L), stir at 40°C for 2 hours, recover the precipitate obtained by the reaction by centrifugal separation, and wash, dry (drying temperature 110°C, drying time 12 hours), grind, and sieve the precipitate, then calcine at 300°C in a muffle furnace for 1 hour, and then perform microwave treatment in a microwave reactor, N2 as the protective gas, the microwave heating temperature is 250°C, the microwave heating frequency is 856-965MHz, and the radiation treatment time is 20 minutes to prepare a NO adsorbent with high adsorption capacity, recorded as 20% MgCo2O4-0.5BaCO3 / AC adsorbent.
[0069] 2. Preparation of microwave catalyst
[0070] The MgCo2O4-40% BaCO3 microwave catalyst was prepared by the preparation method described in the inventor's prior patent document CN201810101669.8.
[0071] 3. Use adsorbent and microwave catalyst to remove NO-containing waste gas
[0072] Experimental equipment: The reactor uses a WG1 / 2.45-Φ5.4×54 quartz tube reactor, the quartz tube is 540mm long and has an inner diameter of 10mm; the microwave power is continuously adjustable from 0 to 1000w, and the frequency is 2400-2500MHz;
[0073] NO x The analyzer is 42C NO-NO2-NO made in the United States x Analyzer.
[0074] In the laboratory, the gas to be treated is a mixture of N2 and NO provided by Dalian Data Gas Co., Ltd., in which the NO concentration is 1000ppm and the oxygen content is 5%.
[0075] Step 3.1, sieving the adsorbent and the microwave catalyst: grinding the 20% MgCo2O4-0.5BaCO3 / AC adsorbent and passing it through a 40-60 mesh sieve to obtain the adsorbent to be loaded; grinding the MgCo2O4-40% BaCO3 microwave catalyst and passing it through a 40-60 mesh sieve to obtain the microwave catalyst to be loaded;
[0076] Step 3.2, loading adsorbent and microwave catalyst: 2 g of adsorbent and 2 g of microwave catalyst are weighed respectively and filled in different positions in the quartz tube of the quartz tube reactor to form an adsorption-microwave catalytic reaction bed, wherein a first section of the bed formed by filling the adsorbent in the quartz tube is arranged adjacent to the air inlet of the quartz tube reactor, and a second section of the bed formed by filling the microwave catalyst in the quartz tube of the quartz tube reactor is arranged adjacent to the air outlet of the quartz tube reactor, and the first section of the bed and the second section of the bed are arranged adjacent to each other;
[0077] Step 3.3, adsorption treatment: passing the gas to be treated into the adsorption-microwave catalytic reaction bed until the NO concentration in the gas at the outlet exceeds 46 ppm (converted according to GB13223-2011 emission standard), wherein the conditions of the adsorption treatment include: residence time 1 s, microwave off, and room temperature;
[0078] Step 3.4 Microwave catalytic treatment: After the adsorption stop condition is reached, the gas passing through the adsorption-microwave catalytic reaction bed is switched to N2, and the microwave catalytic stage is entered. The reaction bed temperature is changed to maintain the bed temperature at 250°C. The microwave equipment automatically adjusts the microwave power. The microwave frequency of the microwave heating treatment is 856-965MHz. The adsorbed NO is desorbed and decomposed into N2 and O2 by microwave catalysis.
[0079] Step 3.5 cyclic reaction: after the adsorbent and microwave catalyst having completed the first adsorption treatment and microwave catalytic treatment are cooled to room temperature, steps 3.3 and 3.4 are repeated in sequence to carry out the second cyclic reaction.
[0080] Figure 1 This is a scanning electron microscope (SEM) image of the 20% MgCo2O4-0.5BaCO3 / AC adsorbent prepared in Example 1 of the present invention. Figure 1 It can be seen that the MgCo2O4 in the 20% MgCO2O4-0.5BaCO3 / AC adsorbent is rich in NO xThe spinel structure of the adsorption site, the rod-like structure of BaCO3, the activated carbon as an adsorption material with a highly developed pore structure, and the MgCO2O4 and BaCO3 dispersed on the surface of the activated carbon, the synergistic effect of the three makes the NO adsorbent have a high adsorption capacity. Figure 2 This is the X-ray diffraction (XRD) spectrum of the 20% MgCo2O4-0.5BaCO3 / AC adsorbent prepared in Example 1 of the present invention. XRD analysis proves that the adsorbent has characteristic diffraction peaks of MgCo2O4 and BaCO3.
[0081] It is necessary to add that Figure 2 The horizontal axis in is 2θ (degrees), Figure 2 The ordinate is intensity (au).
[0082] Figure 3 The schematic diagram of the present invention is to use 20% MgCO2O4-0.5BaCO3 / AC adsorbent and MgCO2O4-40% BaCO3 microwave catalyst to remove NO. Figure 3 As shown, in the first reaction, the adsorption capacity of 20% MgCO2O4-0.5BaCO3 / AC for NO at room temperature was 40.2 mg / g, and when the catalyst bed temperature was 250°C, the conversion rate of microwave catalytic direct decomposition of NO reached more than 99.7%; in the second reaction, the adsorption performance and conversion rate of 20% MgCO2O4-0.5BaCO3 / AC remained stable, indicating that the NO adsorbed on 20% MgCO2O4-0.5BaCO3 / AC was almost desorbed, and could be completely and directly decomposed in the microwave catalytic reaction bed. It can be seen that 20% MgCO2O4-0.5BaCO3 / AC can effectively adsorb NO, and successfully desorb the adsorbed NO at low temperatures.
[0083] Comparative Example 1
[0084] The same as Example 1, except that Mg(NO3)2·6H2O, Co(NO3)2·6H2O and Ba(NO3)2 are not added in step 1.2. The adsorbent used in this example is AC, and the filling amount is 2g, which is recorded as AC adsorbent.
[0085] Calculated based on the time point when the NO outlet concentration exceeded 46 ppm, the adsorption capacity of the AC adsorbent was 9.2 mg / g.
[0086] Comparative Example 2
[0087] The same as Example 1, except that Ba(NO3)2 is not added in step 1.2. The adsorbent used in this example is 20% MgCo2O4 / AC, and the filling amount is 2g, recorded as 20% MgCo2O4 / AC adsorbent, that is, the mass content of MgCo2O4 in the 20% MgCo2O4 / AC adsorbent is 20%.
[0088] Calculated based on the time point when the NO outlet concentration exceeded 46 ppm, the adsorption capacity of 20% MgCo2O4 / AC adsorbent was 9.4 mg / g.
[0089] Comparative Example 3
[0090] The same as Example 1, except that Mg(NO3)2·6H2O and Co(NO3)2·6H2O are not added in step 1.2. The adsorbent used in this example is 20% BaCO3 / AC, and the filling amount is 2g, recorded as 20% BaCO3 / AC adsorbent, that is, the mass content of BaCO3 in the 20% BaCO3 / AC adsorbent is 20%.
[0091] Calculated based on the time point when the NO outlet concentration exceeded 46 ppm, the adsorption capacity of 20% BaCO3 / AC adsorbent was 3.1 mg / g.
[0092] Please refer to Figure 4 and Figure 5 ,in Figure 4 X-ray photoelectron spectroscopy (XPS, O 1s) of the 20% MgCO2O4-0.5BaCO3 / AC adsorbent prepared in Example 1 of the present invention, the 20% MgCO2O4 / AC adsorbent prepared in Comparative Example 2, and the 20% BaCO3 / AC adsorbent prepared in Comparative Example 3. Figure 4 It can be seen that the 20% MgCO2O4-0.5BaCO3 / AC adsorbent has more abundant oxygen vacancies; Figure 5 It can be seen that the adsorption capacity of the adsorbents prepared in Comparative Examples 2 and 3 is lower than that of the adsorbent prepared in Example 1, and insufficient adsorption capacity will lead to frequent system operation and increased operating costs. At the same time, it can also be proved that MgCo2O4, BaCO3 and AC have a synergistic effect.
[0093] Comparative Example 4
[0094] The adsorption capacity data of the adsorbent "NaY-MgCo2O4-40% BaCO3 dual-functional catalytic adsorption material" provided in the patent applied for by the inventor in 2022 (patent application number: CN202211148627.2, patent name: A method for direct decomposition of NO by adsorption-microwave catalysis) is compared with the adsorption capacity data of the 20% MgCO2O4-0.5BaCO3 / AC adsorbent provided in Example 1, see for details. Figure 6 As shown. Figure 6 It can be seen that the adsorption capacity of the 20% MgCO2O4-0.5BaCO3 / AC adsorbent prepared in Example 1 is much higher than that of NaY-MgCo2O4-40% BaCO3.
[0095] Based on the comparison between Example 1 and Comparative Examples 1 to 4, it can be seen that the adsorbent provided in Example 1 can adsorb NO for up to 13 hours within the national emission standards, and its adsorption capacity is as high as 40.2 mg / g. It has the advantage of a long adsorption stage time, and is more efficient and energy-saving compared with related technologies.
[0096] Comparative Example 5
[0097] The same as Example 1, except that in step 3.2, only 20% MgCO2O4-0.5BaCO3 / AC is loaded to form the first bed layer, and no microwave catalyst is loaded.
[0098] like Figure 7 In the first reaction, the adsorption capacity of 20% MgCO2O4-0.5BaCO3 / AC for NO at room temperature was 40.2 mg / g; the adsorbent bed temperature was maintained at 250°C under microwave irradiation, and the desorbed NO was not effectively decomposed, with the outlet concentration being greater than 1950 ppm (the upper limit of NO concentration detected by the instrument is 2000 ppm). Figure 7 It can be seen from the data that the microwave catalytic decomposition ability of 20% MgCO2O4-0.5BaCO3 / AC is poor.
[0099] Example 2
[0100] The same as Example 1, except that the masses of Mg(NO3)2·6H2O, Co(NO3)2·6H2O and Ba(NO3)2 added in step 1.2 are different. The catalyst prepared in Example 2 is recorded as 10% MgCo2O4-0.4BaCO3 / AC.
[0101] Example 3
[0102] The same as Example 1, except that the masses of Mg(NO3)2·6H2O, Co(NO3)2·6H2O and Ba(NO3)2 added in step 1.2 are different. The catalyst prepared in Example 3 is recorded as 20% MgCo2O4-0.4BaCO3 / AC.
[0103] Example 4
[0104] The same as Example 1, except that the masses of Mg(NO3)2·6H2O, Co(NO3)2·6H2O and Ba(NO3)2 added in step 1.2 are different. The catalyst prepared in Example 4 is recorded as 30% MgCo2O4-0.4BaCO3 / AC.
[0105] Example 5
[0106] The same as Example 1, except that the masses of Mg(NO3)2·6H2O, Co(NO3)2·6H2O and Ba(NO3)2 added in step 1.2 are different. The catalyst prepared in Example 5 is recorded as 40% MgCo2O4-0.4BaCO3 / AC.
[0107] The results of NO adsorption capacity and NO conversion rate based on Examples 2 to 5 are plotted as follows: Figure 8 , see Figure 8 , Figure 8 Schematic diagram of NO adsorption capacity of the adsorbent prepared in Examples 2 to 5 of the present invention and the NO conversion rate corresponding to Examples 2 to 5. Figure 8 It can be seen that the adsorption capacities of 10% MgCo2O4-0.4BaCO3 / AC adsorbent, 20% MgCo2O4-0.4BaCO3 / AC adsorbent, 30% MgCo2O4-0.4BaCO3 / AC adsorbent and 40% MgCo2O4-0.4BaCO3 / AC adsorbent are 22.9 mg / g, 31.2 mg / g, 17.1 mg / g and 16.7 mg / g respectively, and the conversion rate of adsorbed NO is greater than 99.5%. When the loading amount of MgCo2O4-BaCO3 is 20%, the adsorption capacity increase effect is most obvious.
[0108] It should be noted that 10%, 20%, 30% and 40% of the horizontal axis correspond to 10% MgCo2O4-0.4BaCO3 / AC adsorbent, 20% MgCo2O4-0.4BaCO3 / AC adsorbent, 30% MgCo2O4-0.4BaCO3 / AC adsorbent and 40% MgCo2O4-0.4BaCO3 / AC adsorbent, respectively, and the bar graph data corresponds to the adsorption capacity of the four adsorbents, and the dots correspond to the NO conversion rates of the four embodiments.
[0109] It is necessary to add that Figure 8 The horizontal axis corresponds to the name of the adsorbent. Figure 8 There are two vertical axes, the left vertical axis corresponds to the adsorption capacity (mg / g), and the right vertical axis corresponds to the NO conversion rate (%).
[0110] Example 6
[0111] The same as Example 1, except that the masses of Mg(NO3)2·6H2O, Co(NO3)2·6H2O and Ba(NO3)2 added in step 1.2 are different. The catalyst prepared in Example 6 is recorded as 20% MgCo2O4-0.3BaCO3 / AC.
[0112] Example 7
[0113] The same as Example 1, except that the masses of Mg(NO3)2·6H2O, Co(NO3)2·6H2O and Ba(NO3)2 added in step 1.2 are different. The catalyst prepared in Example 7 is recorded as 20% MgCo2O4-0.6BaCO3 / AC.
[0114] The results of NO adsorption capacity and NO conversion rate based on Examples 1, 3, 6 and 7 are plotted as follows: Fig. 9 , see Fig. 9 ,from Fig. 9 It can be seen that the adsorption capacities of 20% MgCo2O4-0.3BaCO3 / AC adsorbent, 20% MgCo2O4-0.4BaCO3 / AC adsorbent, 20% MgCo2O4-0.5BaCO3 / AC adsorbent, and 20% MgCo2O4-0.6BaCO3 / AC adsorbent are 21.6 mg / g, 31.2 mg / g, 40.2 mg / g, and 31.1 mg / g, respectively, and the conversion rate of adsorbed NO is greater than 99.5%. With the increase of BaCO3 content, its adsorption capacity gradually increases, and when the BaCO3 content is greater than 0.5, the adsorption capacity decreases. It means that when the BaCO3 content is 0.5, the adsorption capacity increase effect is most obvious.
[0115] It should be noted that 0.3, 0.4, 0.5 and 0.6 on the horizontal axis correspond to 20% MgCo2O4-0.3BaCO3 / AC adsorbent, 20% MgCo2O4-0.4BaCO3 / AC adsorbent, 20% MgCo2O4-0.5BaCO3 / AC adsorbent, and 20% MgCo2O4-0.6BaCO3 / AC adsorbent, respectively, and the bar graph data corresponds to the adsorption capacity of the four adsorbents, and the dots correspond to the NO conversion rates of the four embodiments.
[0116] It is necessary to add that Fig. 9 The horizontal axis corresponds to the name of the adsorbent. Fig. 9 There are two vertical axes, the left vertical axis corresponds to the adsorption capacity (mg / g), and the right vertical axis corresponds to the NO conversion rate (%).
[0117] Example 8
[0118] The same as Example 1, except for the preparation steps of the microwave catalyst, this example adopts the method in the inventor's prior patent document CN201410737055.0 to prepare BaMn 0.9 Mg 0.1 O3 catalyst; the corresponding step 3.1 grinding and sieving is BaMn 0.9 Mg 0.1 O3 catalyst, step 3.2 is loaded with 2g catalyst BaMn 0.9 Mg 0.1 O3.
[0119] That is, compared with Example 1, Example 8 replaces the microwave catalyst from MgCO2O4-40%BaCO3 with BaMn 0.9 Mg 0.1 O3.
[0120] Based on the experimental results of Example 1 and Example 8, Fig.10 ,from Fig.10 It can be seen that MgCO2O4-40%BaCO3, BaMn 0.9 Mg 0.1 O3 can decompose the desorbed NO, indicating that 20% MgCo2O4-0.5BaCO3 / AC adsorbent and a catalyst with high microwave catalytic activity can be combined to achieve the adsorption-microwave catalytic decomposition of NO.
[0121] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions and substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the protection scope of the present invention.
Claims
1. A NO adsorbent, characterized in that: The NO adsorbent is expressed as MgCo2O4-BaCO3 / AC. The MgCo2O4-BaCO3 / AC adsorbent is obtained by loading MgCo2O4 and BaCO3 on the surface of activated carbon particles by coprecipitation. The MgCo2O4 is rich in NO x The spinel structure of the adsorption site, the BaCO3 is a rod-shaped structure, and the synergistic effect of the MgCo2O4, the BaCO3 and the activated carbon makes the NO adsorbent have a high adsorption capacity, wherein the mass ratio of the MgCo2O4-BaCO3:AC is (0.1-0.4):1, and the mass ratio of MgCo2O4:BaCO3 in the MgCo2O4-BaCO3 is 1:(0.1-0.6).
2. The NO adsorbent according to claim 1, characterized in that The mass ratio of the MgCo2O4-BaCO3:AC is (0.1-0.2):1, and the mass ratio of MgCo2O4:BaCO3 in the MgCo2O4-BaCO3 is 1:(0.4-0.6).
3. A method for preparing a NO adsorbent, characterized in that: The preparation method comprises the following steps: (1) dispersing the pretreated activated carbon particles in deionized water to obtain a dispersion; (2) adding Mg(NO3)2, Co(NO3)2 and Ba(NO3)2 to the dispersion in a preset mass ratio, stirring evenly, and then adding a carbonate solution dropwise, stirring at 40-50°C for 1.5-3h, and obtaining a precipitate by solid-liquid separation, and the precipitate is washed, dried, ground, sieved and calcined to obtain a catalyst to be treated; (3) placing the catalyst to be treated in a microwave reactor and treating it under the first preset microwave conditions for 15 to 30 minutes to obtain a MgCo2O4-BaCO3 / AC adsorbent, wherein the mass ratio of the MgCo2O4-BaCO3:AC is (0.1-0.4):1, and the mass ratio of MgCo2O4:BaCO3 in the MgCo2O4-BaCO3 is 1:(0.1-0.6).
4. The method for preparing the NO adsorbent according to claim 3, characterized in that: The first preset microwave conditions in step (3) include: oxygen-free conditions, a microwave heating temperature of 200-400° C., and a microwave frequency of 500-3000 MHz for microwave heating treatment.
5. The method for preparing the NO adsorbent according to claim 3, characterized in that: The calcination conditions in step (2) include: a calcination temperature of 200-350° C. and a calcination time of 1 to 2 hours.
6. The method for preparing the NO adsorbent according to claim 3, characterized in that: The pretreatment step of the activated carbon particles in step (1) includes: dispersing the activated carbon in a KOH solution, stirring at 70-90° C. for 1.5-3 h, filtering after cooling, washing with deionized water until neutral, drying at 100-120° C., and grinding through an 80-mesh sieve to obtain the activated carbon particles.
7. A NO adsorbent, characterized in that: The NO adsorbent is prepared by the preparation method according to any one of claims 3 to 6.
8. Use of the NO adsorbent according to claim 1 or claim 7 in treating waste gas or flue gas containing NO.
9. A method for treating flue gas containing NO, characterized in that: The following steps are included: Filling a NO adsorbent and a microwave catalyst at different positions in a reaction tube of a reactor respectively to form an adsorption-microwave catalytic reaction bed, wherein the NO adsorbent is the NO adsorbent according to claim 1 or claim 7; At least one alternating treatment is used to remove NO from the flue gas, wherein each alternating treatment comprises: passing the flue gas to be treated into the adsorption-microwave catalytic reaction bed, adsorbing NO through the NO adsorbent, and after a preset adsorption time, switching the gas passed into the adsorption-microwave catalytic reaction bed to N2, and under a second preset microwave condition, under the catalytic action of the NO adsorbent and the microwave catalyst, decomposing the NO adsorbed by the NO adsorbent into N2 and O2.
10. The method for treating sintering flue gas containing NO according to claim 9, characterized in that: The microwave catalyst is a MgCo2O4-BaCO3 composite catalyst or a BaMn 0.9 Mg 0.1 O3 catalyst, the second preset microwave conditions include: microwave heating temperature is 100-400°C, and microwave frequency of microwave heating treatment is 500-3000MHz.
Citation Information
Patent Citations
Microwave-catalyzed composite catalysts and their methods for catalytic decomposition of NO
CN108355663B
A method for denitrification by direct decomposition of NO by adsorption-microwave catalysis
CN115445375B
Method for denitration by catalytic direct decomposition of NO with perovskite type catalyst
CN104437079A
Spinel-structured catalyst with capability of simultaneous desulfurization and denitrification as well as preparation method and application of catalyst
CN108355665A
Denitration method for directly decomposing NO through adsorption-microwave catalysis