A low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel and preparation method thereof
By reducing the use of manganese and silicon in the production of hot-rolled duplex steel, and using vacuum induction furnaces and rapid cooling processes, the problems of high cost and unstable tissue performance are solved, and the production of 600MPa grade hot rolling is achieved at low cost and efficiently produced 600MPa grade hot rolling Duplex steel improves the tensile strength and surface quality of the steel plate.
Patent Information
- Application Number
- CN202310417574.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-19
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-04-19
AI Technical Summary
The prior art produces high-strength hot-rolled duplex steel, which has high costs and unstable finished product structure performance, especially due to the high manganese (Mn) content, which leads to increased production costs and difficulty in controlling the cooling process, which affects the final quality of the steel plate.
Using low-cost chemical composition design, the use of manganese (Mn) and silicon (Si) is reduced, and the use of manganese (Mn) and silicon (Si) is prepared through vacuum induction furnace smelting and rolling processes, combined with rapid cooling method, 600MPa grade hot-rolled dual-phase steel is prepared and precious alloys are eliminated. Elements such as molybdenum (Mo) and niobium (Nb) reduce production costs and improve the structural uniformity and surface quality of the steel plate.
Achieve low-cost production of 600MPa-grade hot-rolled dual-phase steel, reducing production costs, improving the tensile strength and yield strength of the steel plate, reducing MnS inclusions, eliminating red iron oxide sheets, simplifying cooling process control, and improving the material Stability of tissue performance.
Smart Images

Figure CN116497274B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy and relates to a low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel and a preparation method thereof. Background Art
[0002] In order to meet the requirements of high safety, the modern automobile manufacturing industry has higher requirements for the strength and formability of automobile plates. Saving production costs and improving production efficiency in the process of producing high-strength automobile plates have become important research directions for major steel companies in the world. Dual-phase steel has excellent formability, a good combination of strength and toughness, and a low yield ratio, which is conducive to reducing the weight of automobiles. The tensile strength of ferrite-martensite dual-phase steel is between 550-650MPa. The chemical composition of hot-rolled dual-phase steel includes alloy elements such as Si, Mn, Ni, and Mo. The use of these elements leads to increased costs or poor surface quality. Low-temperature rolling leads to increased mill pressure, and the complex three-stage cooling method is not only difficult to control, but also affects the stability of the organizational properties of the finished product. Therefore, the production of a low-cost, easy-to-roll high-strength hot-rolled dual-phase steel meets the actual development needs of the automobile manufacturing industry.
[0003] Patent CN200610045846.2 discloses a hot-rolled dual-phase steel plate with a tensile strength of 600 MPa and a manufacturing method thereof. The thickness of the steel plate is 2.5-6 mm. 1.30-1.60% manganese (Mn) and 0.20-0.40% silicon (Si) are added during the composition design. Due to the high manganese (Mn) content (1.30-1.60%), the cost is high and it is easy to cause center segregation of the ingot.
[0004] Patent CN201110303141.7 discloses a 650MPa tensile strength low Si Cr-containing hot-rolled dual-phase steel plate and a manufacturing method thereof. The thickness of the steel plate is 3-10mm. 1.00-1.80% manganese (Mn), 0.05-0.50% silicon (Si) and 0.30-1.50% chromium (Cr) are added during the composition design. Due to the high manganese (Mn) content (1.00-1.80%), the cost is high, and the cooling process is direct laminar cooling with a cooling rate of 20-40°C / s, which easily leads to insufficient ferrite formation.
[0005] Patent CN201310025705.4 discloses a hot-rolled dual-phase steel plate with a tensile strength of 590 MPa and a manufacturing method thereof. The thickness of the steel plate is 2.3 mm. During the composition design, 0.80-2.00% manganese (Mn) may be added, and appropriate amounts of niobium (Nb) and titanium (Ti) may also be added. Due to the high manganese (Mn) content (0.80-2.00%) and the addition of alloying elements, the cost is high. The cooling is carried out in three stages of water cooling-air cooling-water cooling, resulting in poor cooling process control stability, which affects the final organization and performance stability of the material.
[0006] Patent CN200910222583.1 discloses a hot-rolled dual-phase steel plate with a tensile strength of 650 MPa and a manufacturing method thereof. The steel plate adopts (0.05-0.12%) carbon (C) and (0.50-1.20%) silicon (Si) in the composition design, which easily forms red iron oxide scale, resulting in poor surface quality of the steel plate. Summary of the invention
[0007] In view of various deficiencies in the prior art, the present invention provides a low-cost, easy-to-roll 600MPa grade hot-rolled dual-phase steel and a preparation method thereof.
[0008] The invention discloses a low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa, the chemical composition and mass fraction of which include: C: 0.05-0.08%, Si: 0.06-0.09%, Mn: 0.70-1.10%, S: ≤0.015%, P: ≤0.015%, and the balance is Fe and unavoidable impurities.
[0009] The hot-rolled dual-phase steel structure includes a dual-phase structure of ferrite and martensite, the volume fraction of ferrite is 77-91%, the volume fraction of martensite is 9-23%, and the average grain size of ferrite is 3.6-4.1 μm;
[0010] The hot-rolled dual-phase steel has a thickness of 2.0-11 mm, a tensile strength of 608-651 MPa, a yield strength of 352-391 MPa, a yield strength ratio of 0.58-0.60, and an elongation after fracture of 28.9-35.4%.
[0011] A method for preparing a low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel comprises the following steps:
[0012] (1) Using a vacuum induction furnace to melt molten steel and pour it into ingots;
[0013] (2) heating the ingot;
[0014] (3) rolling the ingot in the above step (2) to obtain a plate strip;
[0015] (4) The strip is cooled to obtain 600 MPa grade hot-rolled dual-phase steel.
[0016] The chemical composition of the ingot in step (1) is as follows by mass percentage: C: 0.05-0.08%, Si: 0.06-0.09%, Mn: 0.70-1.10%, S: ≤0.015%, P: ≤0.015%, and the balance is Fe and unavoidable impurities;
[0017] The thickness of the ingot in step (1) is at least 120 mm;
[0018] The heating step (2) is performed at a temperature of 1150 to 1200° C. for a time of 1 to 1.5 h;
[0019] The rolling in step (3) is specifically performed by rolling for 6 to 8 times, with a single-pass reduction rate of 30.0 to 41.1% and a total cumulative reduction rate of 90.8 to 98.3%;
[0020] The starting rolling temperature in step (3) is 1000-1100° C., and the final rolling temperature is 915-960° C.; the thickness of the plate and strip is 2.0-11 mm;
[0021] The cooling described in step (4) is performed at a cooling rate of 80 to 120°C / s and a final cooling temperature of 115 to 200°C.
[0022] The low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel and preparation method of the present invention have the following beneficial effects compared with the prior art:
[0023] (1) Eliminating the precious alloys of molybdenum (Mo), niobium (Nb), and vanadium (V) in steel reduces the amount of manganese (Mn) and silicon (Si) used in steel, significantly reduces production costs, and does not use microalloying elements, which is conducive to the occurrence of ferrite phase transformation after rolling;
[0024] (2) While greatly reducing the amount of manganese (Mn) used in steel, it alleviates the banded structure in the steel, reduces the MnS inclusions in the steel, and improves the uniformity of the steel plate structure and the cold working performance;
[0025] (3) The low silicon (Si) composition design concept eliminates the red iron oxide scale on the surface of the steel plate, and the surface quality of the steel plate is good;
[0026] (4) The rolling temperature is high to prevent low-temperature rolling from placing a heavy burden on the rolling mill. The cooling method of rapid cooling after rolling is used. The simple cooling path is easier to control, and the final material's organizational properties fluctuate less and have better stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A microstructure photograph of the hot-rolled dual-phase steel with a tensile strength of 600 MPa prepared in Example 1 of the present invention after being corroded by LEPERA reagent (1% Na2S2O5 aqueous solution + 4% picric acid alcohol solution);
[0028] Figure 2 The tensile curve of the hot-rolled dual-phase steel with a tensile strength of 600 MPa prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with the embodiments, but the protection scope of the present invention is not limited to the following embodiments.
[0030] Example 1
[0031] A low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa has the following chemical compositions by mass percentage: C: 0.05%, Si: 0.06%, Mn: 1.1%, S: 0.013%, P: 0.015%, and the balance is Fe and unavoidable impurities.
[0032] A method for manufacturing a hot-rolled dual-phase steel with a thickness of 6.0 mm and a tensile strength of 600 MPa, comprising the following process steps:
[0033] (1) Vacuum induction melting is adopted to cast an ingot with a thickness of 120 mm. The chemical composition of the ingot is as follows by mass percentage: C: 0.05%, Si: 0.06%, Mn: 1.1%, S: 0.013%, P: 0.015%, and the balance is Fe and unavoidable impurities. The ingot is heated in a heating furnace for 1.4 h, and the furnace temperature is controlled to be 1170°C;
[0034] (2) The ingot is rolled at a starting rolling temperature of 1100° C. After 7 rolling passes, the reduction passes are distributed as 120 mm→83 mm→53 mm→36 mm→23 mm→14 mm→9.0 mm→6.0 mm, the total cumulative reduction rate is 95.0%, and the final rolling temperature is 960° C., to obtain a plate strip with a thickness of 6.0 mm;
[0035] (3) The strip is rapidly cooled after rolling, with a water cooling rate of 90°C / s and a final cooling temperature of 170°C to obtain a hot-rolled dual-phase steel with a tensile strength of 600 MPa.
[0036] The hot-rolled dual-phase steel with a thickness of 6.0 mm has a dual-phase structure of ferrite and martensite. The microstructure after being corroded by LEPERA reagent (1% Na2S2O5 aqueous solution + 4% picric acid alcohol solution) is shown in the figure. Figure 1 As shown, the volume fraction of ferrite is 84%, the volume fraction of martensite is 16%, the average grain size of ferrite is 3.9μm; the tensile strength is 635MPa, the yield strength is 376MPa, the yield strength ratio is 0.59, and the elongation after fracture is 31.5%.
[0037] Example 2
[0038] A low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa has the following chemical compositions by mass percentage: C: 0.08%, Si: 0.07%, Mn: 0.7%, S: 0.014%, P: 0.014%, and the balance is Fe and unavoidable impurities.
[0039] A method for manufacturing hot-rolled dual-phase steel with a tensile strength of 600 MPa and a thickness of 11 mm, comprising the following process steps:
[0040] (1) Vacuum induction melting is adopted to cast an ingot with a thickness of 120 mm. The chemical composition of the ingot is as follows by mass percentage: C: 0.08%, Si: 0.07%, Mn: 0.7%, S: 0.014%, P: 0.014%, and the balance is Fe and unavoidable impurities. The ingot is heated in a heating furnace for 1 hour, and the furnace temperature is controlled to be 1200°C;
[0041] (2) rolling the ingot at a starting rolling temperature of 1100° C., and rolling the ingot for 6 passes with a reduction pass distribution of 120 mm→83 mm→54 mm→37 mm→25 mm→16 mm→11 mm, a total cumulative reduction rate of 90.8%, and a final rolling temperature of 960° C. to obtain a plate strip with a thickness of 11 mm;
[0042] (3) The strip is rapidly cooled after rolling, with a water cooling rate of 80°C / s and a final cooling temperature of 200°C to obtain a hot-rolled dual-phase steel with a tensile strength of 600 MPa.
[0043] The hot-rolled dual-phase steel with a thickness of 11 mm is a dual-phase structure of ferrite and martensite, in which the volume fraction of ferrite is 77%, the volume fraction of martensite is 23%, and the average grain size of ferrite is 4.1 μm; the yield strength and tensile strength are as follows Figure 2 As shown, the tensile strength is 651 MPa, the yield strength is 391 MPa, the yield strength ratio is 0.60, and the elongation after break is 28.9%.
[0044] Example 3
[0045] A low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa has the following chemical compositions by mass percentage: C: 0.07%, Si: 0.07%, Mn: 0.9%, S: 0.015%, P: 0.013%, and the balance is Fe and unavoidable impurities.
[0046] A method for manufacturing a hot-rolled dual-phase steel with a tensile strength of 600 MPa and a thickness of 2.0 mm, comprising the following process steps:
[0047] (1) Vacuum induction melting is adopted to cast an ingot with a thickness of 120 mm. The chemical composition of the ingot is as follows by mass percentage: C: 0.07%, Si: 0.07%, Mn: 0.9%, S: 0.015%, P: 0.013%, and the balance is Fe and unavoidable impurities. The ingot is heated in a heating furnace for 1.5 h, and the furnace temperature is controlled to be 1150° C.;
[0048] (2) The ingot is rolled at a starting rolling temperature of 1000° C. After 8 rolling passes, the reduction passes are distributed as 120 mm→72 mm→43 mm→26 mm→16 mm→9.5 mm→5.7 mm→3.4 mm→2.0 mm, the total cumulative reduction rate is 98.3%, and the final rolling temperature is 915° C., to obtain a plate strip with a thickness of 2.0 mm;
[0049] (3) The strip is rapidly cooled after rolling, with a water cooling rate of 120°C / s and a final cooling temperature of 115°C to obtain a hot-rolled dual-phase steel with a tensile strength of 600 MPa.
[0050] The hot-rolled dual-phase steel with a thickness of 2.0 mm has a dual-phase structure of ferrite and martensite, in which the volume fraction of ferrite is 91%, the volume fraction of martensite is 9%, and the average grain size of ferrite is 3.6 μm; the tensile strength is 608 MPa, the yield strength is 352 MPa, the yield strength ratio is 0.58, and the elongation after fracture is 35.4%.
[0051] Example 4
[0052] A low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa has the following chemical compositions by mass percentage: C: 0.05%, Si: 0.06%, Mn: 1.1%, S: 0.011%, P: 0.012%, and the balance is Fe and unavoidable impurities.
[0053] A method for manufacturing hot-rolled dual-phase steel with a tensile strength of 600 MPa and a thickness of 8.0 mm comprises the following process steps:
[0054] (1) Vacuum induction melting is adopted to cast an ingot with a thickness of 120 mm. The chemical composition of the ingot is as follows by mass percentage: C: 0.05%, Si: 0.06%, Mn: 1.1%, S: 0.011%, P: 0.012%, and the balance is Fe and unavoidable impurities. The ingot is heated in a heating furnace for 1.2 h, and the furnace temperature is controlled to be 1200° C.;
[0055] (2) The ingot is rolled at a starting rolling temperature of 1080°C. After 7 rolling passes, the reduction passes are distributed as 120 mm → 83 mm → 55 mm → 38 mm → 26 mm → 18 mm → 12 mm → 8.0 mm, the total cumulative reduction rate is 93.3%, and the final rolling temperature is 955°C, to obtain a plate strip with a thickness of 8.0 mm;
[0056] (3) The strip is rapidly cooled after rolling, with a water cooling rate of 120°C / s and a final cooling temperature of 130°C to obtain a hot-rolled dual-phase steel with a tensile strength of 600 MPa.
[0057] The hot-rolled dual-phase steel with a thickness of 8.0 mm has a dual-phase structure of ferrite and martensite, in which the volume fraction of ferrite is 81%, the volume fraction of martensite is 19%, and the average grain size of ferrite is 4.0 μm; the tensile strength is 642 MPa, the yield strength is 381 MPa, the yield strength ratio is 0.59, and the elongation after fracture is 30.7%.
[0058] Example 5
[0059] A low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa has the following chemical compositions by mass percentage: C: 0.06%, Si: 0.09%, Mn: 0.7%, S: 0.014%, P: 0.013%, and the balance is Fe and unavoidable impurities.
[0060] A method for manufacturing a hot-rolled dual-phase steel with a tensile strength of 600 MPa and a thickness of 4.0 mm, comprising the following process steps:
[0061] (1) Vacuum induction melting is adopted to cast an ingot with a thickness of 120 mm. The chemical composition of the ingot is as follows by mass percentage: C: 0.06%, Si: 0.09%, Mn: 0.7%, S: 0.014%, P: 0.013%, and the balance is Fe and unavoidable impurities. The ingot is heated in a heating furnace for 1.5 h, and the furnace temperature is controlled to be 1160° C.;
[0062] (2) The ingot is rolled at a starting rolling temperature of 1010° C. After 8 rolling passes, the reduction passes are distributed as 120 mm→84 mm→54 mm→37 mm→23 mm→15 mm→9.2 mm→6.0 mm→4.0 mm, the total cumulative reduction rate is 96.7%, and the final rolling temperature is 920° C., and a plate strip with a thickness of 4.0 mm is obtained;
[0063] (3) The strip is rapidly cooled after rolling, the water cooling rate is 100°C / s, and the final cooling temperature is 150°C, so as to obtain a hot-rolled dual-phase steel with a tensile strength of 600 MPa.
[0064] The hot-rolled dual-phase steel with a thickness of 4.0 mm has a dual-phase structure of ferrite and martensite, in which the volume fraction of ferrite is 88%, the volume fraction of martensite is 12%, and the average grain size of ferrite is 3.8 μm; the tensile strength is 621 MPa, the yield strength is 366 MPa, the yield strength ratio is 0.59, and the elongation after fracture is 33.2%.
[0065] Example 6
[0066] A low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa has the following chemical compositions by mass percentage: C: 0.08%, Si: 0.08%, Mn: 0.7%, S: 0.015%, P: 0.011%, and the balance is Fe and unavoidable impurities.
[0067] A method for manufacturing hot-rolled dual-phase steel with a tensile strength of 600 MPa and a thickness of 8.0 mm comprises the following process steps:
[0068] (1) Vacuum induction melting is adopted to cast an ingot with a thickness of 120 mm. The chemical composition of the ingot is as follows by mass percentage: C: 0.08%, Si: 0.08%, Mn: 0.7%, S: 0.015%, P: 0.011%, and the balance is Fe and unavoidable impurities. The ingot is heated in a heating furnace for 1.2 h, and the furnace temperature is controlled to be 1155° C.;
[0069] (2) The ingot is rolled at a starting rolling temperature of 1010° C. After 7 rolling passes, the reduction passes are distributed as 120 mm→83 mm→55 mm→38 mm→26 mm→18 mm→12 mm→8.0 mm, the total cumulative reduction rate is 93.3%, and the final rolling temperature is 935° C., and a plate strip with a thickness of 8.0 mm is obtained;
[0070] (3) The strip is rapidly cooled after rolling, with a water cooling rate of 105°C / s and a final cooling temperature of 155°C to obtain a hot-rolled dual-phase steel with a tensile strength of 600 MPa.
[0071] The hot-rolled dual-phase steel with a thickness of 8.0 mm has a dual-phase structure of ferrite and martensite, in which the volume fraction of ferrite is 85%, the volume fraction of martensite is 15%, and the average grain size of ferrite is 3.9 μm; the tensile strength is 625 MPa, the yield strength is 365 MPa, the yield strength ratio is 0.58, and the elongation after fracture is 34.2%.
[0072] Example 7
[0073] A low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa has the following chemical compositions by mass percentage: C: 0.06%, Si: 0.07%, Mn: 0.8%, S: 0.014%, P: 0.012%, and the balance is Fe and unavoidable impurities.
[0074] A method for manufacturing a hot-rolled dual-phase steel with a tensile strength of 600 MPa and a thickness of 10.0 mm, comprising the following process steps:
[0075] (1) Vacuum induction melting is adopted to cast an ingot with a thickness of 120 mm. The chemical composition of the ingot is as follows by mass percentage: C: 0.06%, Si: 0.07%, Mn: 0.8%, S: 0.014%, P: 0.012%, and the balance is Fe and unavoidable impurities. The ingot is heated in a heating furnace for 1.4 h, and the furnace temperature is controlled to be 1165°C;
[0076] (2) The ingot is rolled at a starting rolling temperature of 1010° C. After 6 rolling passes, the reduction passes are distributed as 120 mm→83 mm→54 mm→37 mm→25 mm→16 mm→11 mm, the total cumulative reduction rate is 91.6%, and the final rolling temperature is 953° C., and a plate strip with a thickness of 10.0 mm is obtained;
[0077] (3) The strip is rapidly cooled after rolling, with a water cooling rate of 107°C / s and a final cooling temperature of 166°C to obtain a hot-rolled dual-phase steel with a tensile strength of 600 MPa.
[0078] The hot-rolled dual-phase steel with a thickness of 10.0 mm has a dual-phase structure of ferrite and martensite, in which the volume fraction of ferrite is 80%, the volume fraction of martensite is 20%, and the average grain size of ferrite is 4.1 μm; the tensile strength is 615 MPa, the yield strength is 357 MPa, the yield strength ratio is 0.58, and the elongation after fracture is 33.8%.
[0079] Example 8
[0080] A low-cost, easy-to-roll hot-rolled dual-phase steel with a tensile strength of 600 MPa has the following chemical compositions by mass percentage: C: 0.07%, Si: 0.09%, Mn: 0.9%, S: 0.012%, P: 0.012%, and the balance is Fe and unavoidable impurities.
[0081] A method for manufacturing hot-rolled dual-phase steel with a tensile strength of 600 MPa and a thickness of 8.0 mm comprises the following process steps:
[0082] (1) Vacuum induction melting is adopted to cast an ingot with a thickness of 120 mm. The chemical composition of the ingot is as follows by mass percentage: C: 0.07%, Si: 0.09%, Mn: 0.9%, S: 0.012%, P: 0.012%, and the balance is Fe and unavoidable impurities. The ingot is heated in a heating furnace for 1.2 h, and the furnace temperature is controlled to be 1170°C;
[0083] (2) The ingot is rolled at a starting rolling temperature of 1010° C. After 7 rolling passes, the reduction passes are distributed as 120 mm→83 mm→55 mm→38 mm→26 mm→18 mm→12 mm→8.0 mm, the total cumulative reduction rate is 93.3%, and the final rolling temperature is 957° C., to obtain a plate strip with a thickness of 8.0 mm;
[0084] (3) The strip is rapidly cooled after rolling, with a water cooling rate of 97°C / s and a final cooling temperature of 138°C to obtain a hot-rolled dual-phase steel with a tensile strength of 600 MPa.
[0085] The hot-rolled dual-phase steel with a thickness of 8.0 mm has a dual-phase structure of ferrite and martensite, in which the volume fraction of ferrite is 79%, the volume fraction of martensite is 21%, and the average grain size of ferrite is 3.6 μm; the tensile strength is 640 MPa, the yield strength is 377 MPa, the yield strength ratio is 0.59, and the elongation after fracture is 30.2%.
Claims
1. A low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel, It is characterized in that The chemical composition and mass fraction of the hot-rolled dual-phase steel include: C: 0.05-0.08%, Si: 0.06-0.09%, Mn: 0.70-1.10%, S: ≤0.015%, P: ≤0.015%, and the balance is Fe and unavoidable impurities; The hot-rolled dual-phase steel comprises ferrite and martensite, wherein the volume fraction of ferrite is 77-91%, and the volume fraction of martensite is 9-23%; the average grain size of ferrite is 3.6-4.1 μm; The hot-rolled dual-phase steel has a tensile strength of 608-651 MPa, a yield strength of 352-391 MPa, a yield strength ratio of 0.58-0.60, and an elongation after fracture of 28.9-35.4%.
2. The low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel according to claim 1, It is characterized in that The thickness of the hot-rolled dual-phase steel is 2.0-11 mm.
3. A method for preparing the low-cost, easy-to-roll 600MPa grade hot-rolled dual-phase steel according to claims 1 to 2, It is characterized in that The following steps are involved: (1) Using a vacuum induction furnace to melt molten steel and pour it into ingots; (2) heating the ingot; (3) rolling the ingot in the above step (2) to obtain a plate strip; (4) cooling the strip to obtain 600 MPa grade hot-rolled dual-phase steel; In the step (3), the starting rolling temperature is 1000-1100° C., and the final rolling temperature is 915-960° C.; the thickness of the plate and strip is 2.0-11 mm; In the step (4), the cooling rate is 80-120°C / s, and the final cooling temperature is 115-200°C.
4. The method for preparing the low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel according to claim 3, It is characterized in that The chemical composition of the ingot in step (1) is as follows by mass percentage: C: 0.05-0.08%, Si: 0.06-0.09%, Mn: 0.70-1.10%, S: ≤0.015%, P: ≤0.015%, and the remainder is Fe and unavoidable impurities.
5. The method for preparing the low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel according to claim 3, It is characterized in that The thickness of the ingot in step (1) is at least 120 mm.
6. The method for preparing the low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel according to claim 3, It is characterized in that The heating is performed as described in step (2), the heating temperature is 1150-1200° C., and the heating time is 1-1.5 h.
7. The method for preparing the low-cost and easy-to-roll 600MPa grade hot-rolled dual-phase steel according to claim 3, It is characterized in that The rolling in step (3) is specifically performed by rolling 6 to 8 times, with a single-pass reduction rate of 30.0 to 41.1% and a total cumulative reduction rate of 90.8 to 98.3%.
Citation Information
Patent Citations
650MPa-level low-Si Cr-containing hot-rolled dual phase steel plate and manufacturing method thereof
CN103031493B
Five hundred and ninety Mpa-grade dual-phase steel and production method thereof
CN103088258A
Tensile strength 600Mpa grade dual phase steel plate and its production method
CN1807669A
Hot rolled dual phase steel plate with 650MPa of tensile strength and manufacturing method thereof
CN101717886A
High strength steel plate excellent in formability and method for production thereof
CN1788099A