Phase change building material and preparation method and application thereof
By incorporating pore-forming particles into building materials and immersing them in a phase change solution to prepare porous phase change materials, the problems of leakage and corrosion of inorganic phase change materials in buildings are solved, achieving uniform distribution and efficient heat storage performance of phase change materials, and simplifying the operation process.
Patent Information
- Application Number
- CN202310579458.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-17
AI Technical Summary
In the existing technology, inorganic phase change materials have problems of leakage and corrosion when used in buildings, and the preparation process is complicated, making it difficult to achieve good compatibility and uniform distribution with building materials.
By incorporating pore-forming particles into the slurry to form a porous solid material, and then immersing it in a phase change solution, the phase change material is uniformly distributed within the interconnected pores. Combined with magnesium oxide, a leak-proof shell is formed, thus preparing a porous phase change building material.
It achieves uniform distribution of phase change materials, improves heat storage performance and thermal conductivity, prevents leakage, simplifies operation procedures, and reduces economic costs.
Smart Images

Figure CN116514522B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building materials, and in particular relates to a phase change building material and a preparation method and application thereof. Background Art
[0002] Building energy consumption accounts for a considerable proportion of energy consumption in various fields. my country's direct or indirect building energy consumption is very huge. Therefore, reducing building energy consumption and improving energy efficiency are the only way to achieve energy conservation. Phase change material (PCM-Phase Change Material) refers to a substance that changes the state of matter and can provide latent heat when the temperature remains unchanged. The combination of phase change materials with heat storage function and building materials and their application in the construction field is a revolutionary development in the construction field, which can effectively reduce energy consumption and achieve the purpose of energy conservation. Phase change energy storage materials are added to building components, which absorb heat when the temperature is too high and release heat when the temperature is too low, so that the building components undergo phase change according to the changes in room temperature, thereby automatically adjusting the indoor temperature. Compared with traditional building materials, phase change energy storage building materials have the advantages of obvious heat storage effect and more environmental protection.
[0003] According to the phase change form of phase change materials, they can be divided into solid-solid, solid-liquid, solid-gas and liquid-gas energy storage phase change materials. Among them, solid-liquid phase change materials have become a hot research topic due to their advantages such as nearly constant temperature in the phase change process, wide phase change temperature range, small volume change rate and low cost. Phase change energy storage materials can be divided into organic and inorganic phase change materials according to the properties of the materials themselves. Organic phase change materials mainly include paraffin and non-paraffin. Inorganic phase change materials mainly include crystalline hydrated salts, molten salts and metal alloys. Inorganic phase change materials are widely used because of their low price, high thermal storage density and large latent heat of phase change.
[0004] Phase change energy storage materials are generally difficult to use directly when used as building materials. In most cases, they need to be formed into a solid shape or a non-leaking composite material. At present, the application methods of phase change energy storage materials in construction include: ① directly immersing the phase change material into the pores of the building material or adding it to the building material as a filler. For example, Chinese invention patent CN1303181C discloses a phase change energy storage composite material for construction and a preparation method thereof. The method uses air-hardening or water-hardening gelling materials such as gypsum and cement as a matrix, in which porous material aggregates such as expanded clay are dispersed, and organic phase change materials such as paraffin or butyl stearate are stored in the porous material aggregate. The method uses a vacuum infiltration method to prepare a phase change energy storage aggregate, and then uses a general method for building materials to prepare a phase change energy storage composite material. ② The phase change material is prepared into a shaped phase change material or encapsulated into a monomer and then combined with the building material. For example, Chinese invention patent CN113175174B discloses a phase-change heat storage board for construction, which encapsulates phase-change material particles inside the building board so that the building board has the function of heat storage and heat release. The first method is simple to operate, but the surface of the component is prone to obvious leakage during the phase change process, and the safety and stability are poor, which is not conducive to long-term use. The second method avoids direct contact between the phase change material and traditional building materials, which can effectively realize latent heat storage and improve the stability of application, but the process of shaping the phase change material or encapsulating it into a monomer is relatively complicated, which is not conducive to promotion considering the packaging cost, operation process, economy, etc.
[0005] In summary, the direct infiltration or incorporation of phase change energy storage materials into building materials is the focus of future development. Inorganic phase change materials are the most widely used type of phase change materials and are also typical solid-liquid phase change materials. Compared with organic phase change materials, they are widely available and inexpensive, have no pungent odor, and have stable chemical properties, making them more suitable for use in the field of building energy conservation. However, inorganic phase change materials have the defects of supercooling and phase separation, which limits their application. Secondly, most inorganic phase change materials are hydrated salts. When combined with traditional building materials, they will not only cause direct leakage problems, but also corrode the base material over a long period of time, causing leakage or failure of the phase change material. Therefore, it is urgent to provide a method for preparing phase change building materials to solve these problems. Summary of the invention
[0006] In view of the technical problems existing in the prior art, the present invention provides a phase change building material and a preparation method and application thereof, with the aim of preparing a phase change building material with good workability, better thermal conductivity, good compatibility between the phase change material and the building material, and uniform distribution of the phase change material through a simple preparation method.
[0007] To achieve the above objectives, the present invention provides the following technical solutions.
[0008] A preparation method of a phase change building material and its application, the preparation method comprising: adding pore-forming particles into a slurry, forming a solid phase material after solidification treatment, dissolving or melting the pore-forming particles and discharging them from the solid phase material to obtain a porous solid phase material with interconnected pores inside; immersing the porous solid phase material in a phase change solution to obtain a phase change building material in which the interconnected pores are filled with the phase change solution.
[0009] Further, the solid phase material is crushed into solid phase granular material, and the pore-forming particles are discharged from the solid phase granular material by dissolving or melting to obtain a porous solid phase granular material with interconnected pores inside; the porous solid phase granular material is immersed in a phase change solution to obtain a phase change building material in which the interconnected pores are filled with the phase change solution, and the phase change building material is mixed with the slurry and injected into a mold;
[0010] Furthermore, the particle size of the solid phase granular material is 2-3 cm.
[0011] Furthermore, the pore diameter of the connecting holes is between 0.5-10 mm, and the average pore diameter is between 2-5 mm, so that the phase change material is evenly distributed, thereby improving the heat storage and heat release performance.
[0012] Furthermore, the slurry is MPC slurry.
[0013] Furthermore, the MPC slurry is prepared by mixing dead-burned magnesium oxide, ammonium dihydrogen phosphate and borax in a mass ratio of 1.5:1:0.1 and then adding water.
[0014] Furthermore, magnesium oxide is adsorbed on the surface of the phase change building material to form a leakage-proof shell, which is then mixed with the slurry and injected into a mold.
[0015] Furthermore, the slurry includes any one of MOC slurry and MOS slurry.
[0016] Furthermore, the MOC slurry is formed by mixing active magnesium oxide and magnesium chloride solution; and the MOS slurry is formed by mixing active magnesium oxide and magnesium sulfate solution.
[0017] Furthermore, the active magnesium oxide is calcined from any one of dolomite, magnesite, and magnesite, or a combination of two or more thereof.
[0018] Furthermore, the active content of the active magnesium oxide is between 20% and 80%.
[0019] Furthermore, the pore-forming particles include soluble or fusible salts.
[0020] Furthermore, the amount of the pore-forming particles added is 10-80% of the mass of the slurry.
[0021] Furthermore, the solid-phase particle material is immersed in water or an organic solvent so that the pore-forming particles are dissolved and then discharged; or the solid-phase particle material is heated so that the pore-forming particles are melted and discharged.
[0022] Furthermore, the solute of the salt solution is the same as the salt forming the pore-forming particles.
[0023] Furthermore, the organic solvent includes any one of ethanol and methanol.
[0024] Furthermore, the soluble or molten salt includes any one of sodium chloride, carnallite, magnesium chloride hexahydrate, calcium chloride hexahydrate, magnesium sulfate heptahydrate, potassium dihydrogen phosphate, and ammonium dihydrogen phosphate.
[0025] Furthermore, the phase change solution includes one of calcium chloride hexahydrate and magnesium chloride hexahydrate, or a combination of the two, or a phosphate solution.
[0026] Furthermore, a nucleating agent or stabilizer is added to the phase change solution, and the nucleating agent can be any one of boric acid, SrCl2·6H2O, SrCO3, hydroxyethyl cellulose (HEC), polyacrylamide (PAM), sodium polyacrylate (PAAS) or a combination of two or more thereof.
[0027] The phase change building material prepared based on the above preparation method can form a porous phase change building material that does not react with the phase change material, and the phase change material is evenly distributed in the porous material.
[0028] The phase change building material prepared by the invention is applied in the construction industry.
[0029] Compared with the prior art, the present invention has at least the following beneficial effects:
[0030] 1. The phase change building material obtained by adopting the technical solution of the present invention can form a porous material that does not react with the phase change material. The phase change material is evenly distributed in the porous material. The pore size of the connecting pores is between 0.5-10mm, and the average pore size is 2-5mm, so that the phase change material is evenly distributed, the heat storage and heat release performance is improved, the thermal conductivity is enhanced, and the leakage of the phase change material is effectively prevented.
[0031] 2. The gelling material is consistent with the phase change material and the packaging material, and has good workability. The same materials are more conducive to forming a whole, improving the supercooling and phase separation problems of the phase change material.
[0032] 3. The present invention can be regarded as a perfect combination of direct incorporation method and encapsulation method based on the same type of materials, with simple actual operation and low economic cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0034] Figure 1 It is a schematic cross-sectional diagram of the salt-containing granular MOC concrete particles in Example 2 of the present application.
[0035] Figure 2 It is a schematic cross-sectional view of the salt-containing MOC concrete particles after immersion in Example 2 of the present application.
[0036] Figure 3 It is a schematic diagram of interconnected pores formed after the salt-containing granular MOC concrete particles in Example 2 of the present application are immersed. DETAILED DESCRIPTION
[0037] The present invention will be more fully understood through the following detailed description, which should be read in conjunction with the accompanying drawings. Detailed embodiments of the present invention are disclosed herein; however, it should be understood that the disclosed embodiments are only exemplary of the present invention, which can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be interpreted as limiting, but only as the basis of the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in virtually any appropriate detailed embodiment.
[0038] The various aspects, embodiments, features and examples of the present invention should be considered as illustrative in all aspects and are not intended to limit the present invention, the scope of the present invention is defined only by the claims. Other embodiments, modifications and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.
[0039] Example 1
[0040] This embodiment provides a magnesium phosphate-based concrete phase change building material, and the preparation method is as follows:
[0041] 1. Preparation of MPC Slurry
[0042] Dead-burned magnesium oxide, ammonium dihydrogen phosphate and borax were uniformly mixed in a mass ratio of 1.5:1:0.1 and ball-milled to prepare an MPC dry powder mixture, and 0.65 times by mass of water was added to the MPC dry powder mixture to form an MPC slurry.
[0043] 2. Add salt particles into MPC slurry
[0044] Weigh sodium chloride particles with a mass that is 50% of the mass of the MPC slurry in step 1, and mix them evenly with the MPC slurry obtained in step 1 to form an MPC slurry containing salt particles.
[0045] The salt-containing particle slurry was cured at room temperature for 1 day to obtain the salt-containing particle MPC concrete.
[0046] 3. The salt-containing MPC concrete blocks in step 2 are crushed and sieved into particles of 0.5-5 cm.
[0047] 4. Select the salt-containing MPC coagulation particles with a particle size of 2-3 cm after the particles are crushed in step 3 and soak them in water for 3 days to dissolve and leach the sodium chloride particles inside. Pores will be formed at the locations where the original sodium chloride particles were located. After the sodium chloride particles are dissolved and leached, the adjacent pore walls will be interconnected. The MPC substrate will be hydrated and decomposed in the water environment, so that the pores are connected to each other to form interconnected pores.
[0048] 5. The MPC concrete particles with interconnected pores formed inside obtained in step 4 are immersed in a phase change solution of sodium hydrogen phosphate dodecahydrate (Na2HPO4·12H2O) to fill the internal interconnected pores with the phase change material to form X-MPC particles containing the phase change material.
[0049] 6. The dead-burned magnesium oxide, diammonium phosphate, borax and X-MPC particles are uniformly mixed in a mass ratio of 1.5:1:0.1:2, water is added to the mixture to form a slurry, the mixture is stirred evenly and injected into a mold to form magnesium phosphate-based concrete phase change building materials of different sizes.
[0050] When applied to the construction field, compared with phase change building materials prepared by traditional methods (i.e., direct incorporation or infiltration), the phase change material is evenly distributed in the connected pores, so that the phase change building material has high thermal conductivity and no leakage.
[0051] Example 2
[0052] This embodiment provides a magnesium oxychloride-based concrete phase change building material. Specifically, the preparation method is as follows:
[0053] 1. Preparation of MOC slurry
[0054] Magnesium chloride is dissolved in water to prepare a magnesium chloride solution with a concentration of 25%, and then mixed evenly with active magnesium oxide powder (activity 10%) to form MOC slurry.
[0055] 2. Add salt particles into MOC slurry
[0056] Weigh MgCl2·6H2O particles with a mass of 40% of the mass of the MOC slurry in step 1, and mix them evenly with the MOC slurry obtained in step 1 to form a MOC slurry containing salt particles.
[0057] The salt-containing particle slurry was cured at room temperature for 3 days and then dried at 50° C. for 6 h to obtain dried salt-containing particle MOC concrete.
[0058] See also Figure 1 , is a schematic cross-sectional view of the salt-containing particle MOC concrete block of this embodiment, where it can be seen that the MgCl2·6H2O particles are wrapped in the MOC matrix.
[0059] 3. The salt-containing MOC concrete blocks dried in step 2 are crushed and sieved into particles of 0.5-5 cm.
[0060] 4. Select the salt-containing MOC concrete particles with a particle size of 2-3 cm in step 3 and soak them in a 15% magnesium chloride solution for 3 days to dissolve and leach the MgCl2·6H2O particles inside. Pores will be formed at the locations where the salt particles were originally located. After the salt particles melt and leach, the adjacent pore walls will be interconnected to form connected pores together with the pores.
[0061] See also Figure 2 , Figure 2 is a schematic cross-sectional view of the salt-containing MOC concrete particles in Example 2 of the present application after immersion, where pores are formed at the locations where the MgCl2·6H2O particles were originally located, and there are pore walls between adjacent pores; Figure 3 , Figure 3 This is a schematic diagram of the connected pores formed after the salt-containing MOC concrete particles in Example 1 of the present application are soaked. It can be seen that the pore walls between adjacent pores are interconnected, and together with the pores, a connected pore is formed. The pore diameter of the connected pore is between 0.5-10mm, and the average pore diameter is 2-5mm, so that the phase change material is evenly distributed, and the heat storage and heat release performance is improved.
[0062] 5. The MOC concrete particles with interconnected pores obtained in step 4 are immersed in a mixed phase change solution of calcium chloride (CaCl2·6H2O) and magnesium chloride (MgCl2·6H2O) so that the internal interconnected pores are filled with phase change materials to form X-MOC particles containing phase change materials.
[0063] 6. Dry the X-MOC particles obtained in step 5 at 50°C to remove excess water, so that the moisture content is 30%.
[0064] 7. The X-MOC particles dried in step 6 with a moisture content of 30% are adsorbed in magnesium oxide powder. The surface of the X-MOC adsorbed with magnesium oxide particles will be coated with a layer of MOC to form MX-MOC particles. The MX-MOC particles are placed at room temperature for 3 days to stabilize them.
[0065] 8. Dissolve magnesium chloride in water to prepare a magnesium chloride solution (concentration 30%), mix it with active magnesium oxide powder (activity 60%) and stir it evenly to form MOC slurry, then mix it with MX-MOC particles in the MOC slurry, the mass ratio of slurry to particles is 1:0.5, stir it evenly and inject it into a mold to form magnesium oxychloride-based concrete phase change building materials of different sizes.
[0066] Example 3
[0067] This embodiment provides a phase change concrete energy storage material for construction, and the preparation method is as follows:
[0068] 1. Preparation of MOC slurry
[0069] Magnesium chloride is dissolved in water to prepare a magnesium chloride solution (concentration 27%), which is evenly mixed with active magnesium oxide powder (activity 60%) to form MOC slurry.
[0070] 2. Add salt particles into MOC slurry
[0071] Weigh sodium chloride particles whose mass is 50% of the mass of the MOC slurry in step 1, and mix them evenly with the MOC slurry obtained in step 1 to form a MOC slurry containing salt particles.
[0072] The salt-containing particle slurry was cured at room temperature for 7 days and then dried at 50°C for 12 hours to obtain oven-dried salt-containing particle MOC concrete.
[0073] 3. The salt-containing MOC concrete blocks dried in step 2 are crushed and sieved into particles of 0.5-5 cm.
[0074] 4. Soak the salt-containing particle MOC concrete block after the particles are crushed in step 3 in water for 5 days to melt and leach the sodium chloride particles inside. Pores will be formed at the original locations of the sodium chloride particles. After the sodium chloride particles melt and leach, the adjacent pore walls will be interconnected to form connected pores together with the pores.
[0075] 5. A nucleating agent is added to the CaCl2·6H2O phase change solution to form a mixed solution. For example, the nucleating agent can be any one of boric acid, SrCl2·6H2O, SrCO3, hydroxyethyl cellulose (HEC), polyacrylamide (PAM), sodium polyacrylate (PAAS), or a combination of two or more thereof.
[0076] The MOC concrete particles with interconnected pores obtained in step 4 are immersed in the mixed solution, so that the internal interconnected pores are filled with phase change materials to form X-MOC particles containing phase change materials.
[0077] 6. The X-MOC particles obtained in step 5 are dried at 50° C. or at rest to remove excess water, so that the moisture content is 40%.
[0078] 7 After drying in step 6, the X-MOC particles with a moisture content of 40% are adsorbed in magnesium oxide powder. The surface of the X-MOC adsorbed with magnesium oxide particles will be coated with a layer of MOC to form MX-MOC particles. The MX-MOC particles are placed at room temperature for 7 days to stabilize them.
[0079] 8. Dissolve magnesium chloride in water to prepare a magnesium chloride solution with a concentration of 20%, mix it with active magnesium oxide powder (activity 60%) and stir it evenly to form MOC slurry, then mix it with MX-MOC particles in the MOC slurry, stir it evenly and inject it into the mold to form phase change building materials of different sizes.
[0080] Example 4
[0081] This embodiment provides a phase change concrete energy storage material for construction, and the preparation method is as follows:
[0082] 1. Preparation of MOS slurry
[0083] Magnesium sulfate is dissolved in water to prepare a magnesium sulfate solution with a concentration of 25%, and then mixed evenly with active magnesium oxide powder (activity 80%) to form MOS slurry.
[0084] 2. Add salt particles into MOS slurry
[0085] Weigh MgSO4·7H2O particles with a mass of 40% of the mass of the MOS slurry in step 1, and mix them evenly with the MOS slurry obtained in step 1 to form a MOS slurry containing salt particles.
[0086] The salt-containing particle slurry was cured at room temperature for 3 days and then dried at 50° C. for 6 days to obtain dried salt-containing particle MOS concrete.
[0087] 3. The salt-containing MOS concrete blocks dried in step 2 are crushed and sieved into particles of 0.5-5 cm.
[0088] 4. Select the salt-containing MOS coagulated particles with a particle size of 2-3 cm after the particles are crushed in step 3 and soak them in a 5% magnesium sulfate solution for 5 days to melt and leach the MgSO4·7H2O particles inside. Pores will be formed at the locations where the original MgSO4·7H2O particles were located. After the MgSO4·7H2O particles are melted and leached, the nearby pore walls will be interconnected. The MOS substrate will be hydrated and decomposed in the water environment, so that the pores are connected to each other to form interconnected holes.
[0089] 5. The MOS concrete particles with interconnected pores formed inside obtained in step 4 are immersed in a Na2SO4·10H2O phase change solution, so that the internal interconnected pores are filled with phase change materials to form X-MOS particles containing phase change materials.
[0090] 6. The X-MOC particles obtained in step 5 are dried at 50°C to remove excess water, so that the moisture content is 30-40%.
[0091] 7. The X-MOS particles dried in step 6 are adsorbed in magnesium oxide powder. The surface of the X-MOC adsorbed with magnesium oxide particles will be coated with a layer of MOS to form MX-MOS particles. The MX-MOS particles are placed at room temperature for 3 days to stabilize them.
[0092] 8. Dissolve magnesium sulfate in water to prepare a 30% magnesium sulfate solution, mix it with active magnesium oxide powder (activity 60%) and stir it evenly to form MOS slurry, then mix it with MX-MOS particles in the MOS slurry, stir it evenly and inject it into a mold to form phase change building materials of different sizes.
[0093] Example 5
[0094] The only difference between this embodiment and embodiment 2 is that in step 2 of this embodiment, 10% of the mass of carnallite in the MOC slurry in step 1 is weighed and mixed evenly with the MOC slurry obtained in step 1 to form a MOC slurry containing salt particles. The other conditions are the same as those in embodiment 2.
[0095] Example 6
[0096] The only difference between this embodiment and embodiment 2 is that in step 2 of this embodiment, magnesium chloride hexahydrate of 80% of the mass of the MOC slurry in step 1 is weighed and evenly mixed with the MOC slurry obtained in step 1 to form a MOC slurry containing salt particles. The other conditions are the same as those in embodiment 2.
[0097] Example 7
[0098] The only difference between this embodiment and embodiment 2 is that in step 2 of this embodiment, potassium dihydrogen phosphate accounting for 20% of the mass of the MOC slurry in step 1 is weighed and evenly mixed with the MOC slurry obtained in step 1 to form a MOC slurry containing salt particles. The other conditions are the same as those in embodiment 2.
[0099] Example 8
[0100] The only difference between this embodiment and embodiment 2 is that in step 2 of this embodiment, ammonium dihydrogen phosphate accounting for 70% of the mass of the MOC slurry in step 1 is weighed and evenly mixed with the MOC slurry obtained in step 1 to form a MOC slurry containing salt particles. The other conditions are the same as those in embodiment 2.
[0101] Example 9
[0102] The only difference between this embodiment and embodiment 2 is that heating is performed to melt and leach the internal MgCl2·6H2O particles. The other conditions are the same as those in embodiment 2.
[0103] Example 10
[0104] The only difference between this embodiment and embodiment 2 is that the salt-containing MOC concrete particles with a particle size of 2-3 cm in step 3 are selected and immersed in ethanol for 3 days to dissolve and leach the MgCl2·6H2O particles inside. The other conditions are the same as those in embodiment 2.
[0105] The ethanol in this embodiment can be replaced by other alcohol organic solvents such as methanol.
[0106] The invention provides a preparation method of a phase change building material. The building material is formed by mixing selected salt particles into a slurry and curing the slurry. The salt particles in the building material are then dissolved by immersion or heated to melt so that the selected particles are discharged from the interior of the building material to form interconnected holes. The building material with interconnected holes is immersed in a phase change solution so that the phase change solution is evenly distributed in the interconnected holes to form phase change building particles. In some embodiments, magnesium oxide is adsorbed on the surface of the phase change building particles to form a leakage-proof shell. The combination of the new building material formed by mixing salt and active magnesium oxide into a slurry and then oxidizing the slurry and the inorganic phase change material solves the problem of poor compatibility between traditional building materials and inorganic phase change materials. The method of encapsulating the phase change material and then infiltrating it into a gelling matrix to form the phase change building material combines the advantages of the infiltration method and the encapsulation method, is simple to operate, highly economical, and has strong leakage resistance. The phase change material, encapsulation material, and gelling matrix formed by the same materials make the workability of the phase change building material better.
[0107] Although the present invention has been described with reference to illustrative embodiments, it will be appreciated by those skilled in the art that various other changes, omissions and / or additions may be made and that elements of the described embodiments may be substituted with substantial equivalents without departing from the spirit and scope of the present invention. In addition, many modifications may be made to adapt a particular situation or material to the teachings of the present invention without departing from the scope of the present invention. Therefore, it is not intended herein to limit the present invention to the specific disclosed embodiments for carrying out the present invention, but rather it is intended that the present invention will include all embodiments within the scope of the appended claims.
Claims
1. A method for preparing a phase change building material, characterized in that include: Adding pore-forming particles into the slurry, forming a solid phase material after solidification treatment, breaking the solid phase material into solid phase granular material, and then dissolving or melting the pore-forming particles and discharging them from the solid phase granular material to obtain a porous solid phase granular material with interconnected pores inside; immersing the porous solid phase granular material in a phase change solution to obtain a phase change building material in which the interconnected pores are filled with the phase change solution; Adsorbing magnesium oxide on the surface of the phase change building material to form a leak-proof shell, and then mixing it with the slurry and injecting it into a mold; The slurry includes any one of MOC slurry and MOS slurry, or the slurry is MPC slurry, the MOC slurry is formed by mixing active magnesium oxide and magnesium chloride solution, the MOS slurry is formed by mixing active magnesium oxide and magnesium sulfate solution, and the MPC slurry is formed by mixing dead-burned magnesium oxide, diammonium hydrogen phosphate and borax in a mass ratio of 1.5:1:0.1 and then adding water.
2. The method for preparing a phase change building material according to claim 1, characterized in that: The particle size of the solid phase granular material is 2-3 cm.
3. The method for preparing the phase change building material according to claim 1, characterized in that: The active magnesium oxide is calcined by calcining any one of dolomite, magnesite and magnesite or a combination of two or more thereof.
4. The method for preparing a phase change building material according to claim 1, characterized in that: The pore-forming particles include soluble or fusible salts; And / or, the amount of the pore-forming particles added is 10-80% of the mass of the slurry.
5. The method for preparing the phase change building material according to claim 4, characterized in that: Immersing the solid phase particle material in water, salt solution or organic solvent so that the pore-forming particles are dissolved and then discharged; And / or, heating is performed so that the pore-forming particles are melted and discharged.
6. The method for preparing the phase change building material according to claim 5, characterized in that: The solute of the salt solution is the same as the salt forming the pore-forming particles; And / or, the organic solvent includes any one of ethanol and methanol.
7. The method for preparing a phase change building material according to claim 4, characterized in that: The soluble or molten salt includes any one of sodium chloride, carnallite, magnesium chloride hexahydrate, calcium chloride hexahydrate, magnesium sulfate heptahydrate, potassium dihydrogen phosphate, and ammonium dihydrogen phosphate.
8. The method for preparing the phase change building material according to claim 5, characterized in that: The phase change solution includes one of calcium chloride hexahydrate, magnesium chloride hexahydrate, or a combination of the two, or a phosphate solution; And / or, a nucleating agent or a stabilizing agent is added to the phase change solution.
9. A phase change building material prepared by the method for preparing a phase change building material according to any one of claims 1 to 8.
10. Use of the phase change building material according to claim 9 in the field of construction.