A rubber particle modifier for rubber concrete and preparation method thereof

By spraying modifiers such as epoxy resin on the surface of rubber particles, the compressive strength of rubber concrete is improved by spraying epoxy binders and dual chemical bonds, and the problem of insufficient bonding strength between rubber particles and cement matrix in the prior art is solved. , realizes simple and efficient rubber concrete modification, and promotes the widespread application of rubber concrete in engineering applications.

CN116535125BActive Publication Date: 2024-12-06NORTH CHINA UNIV OF WATER RESOURCES & ELECTRIC POWER
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310548774.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-12-06
Estimated Expiration
2043-05-16

AI Technical Summary

Technical Problem

The compressive strength of existing rubber concrete is low, mainly due to the insufficient bonding strength between rubber particles and cement matrix, resulting in a decrease in the concrete strength. The existing modification methods have little effect on the washing treatment, cumbersome and dangerous modification of NaOH solution. The problem of complex and high cost in silane-modified polymer emulsions.

Method used

Using a rubber particle modifier, including epoxy resin, Tween, primer solution, OP-10, polyvinyl alcohol and silane coupling agent, the rubber particle surface is sprayed to form a strong effect with the cement matrix. Bonding, use epoxy adhesives and bisexual chemical bonds to improve the bonding effect.

Benefits of technology

It significantly improves the compressive strength of rubber concrete, has a simple modification process and high cost performance, and basically does not affect the foundation performance of concrete. It is of practical significance to promote the application of rubber concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004230580780000061
    Figure BDA0004230580780000061
Patent Text Reader

Abstract

The present invention belongs to the technical field of building materials, and specifically relates to a rubber particle modifier for rubber concrete and a preparation method thereof. The rubber particle modifier contains Z44, Tween, CS-20, OP-10, polyvinyl alcohol, KH570 and ethanol solution. Modifier preparation process: first, Tween, CS-20, and OP-10 are mixed and added to Z44, and stirred to form a mixed solution I; then polyvinyl alcohol is added to the mixed solution I, and stirred to form a mixed solution II; finally, KH570 is added to the mixed solution II, and then an ethanol solution is added, and stirred to form a mixed solution III, which is a rubber particle modifier. When in use, the rubber particle modifier is evenly sprayed onto the surface of the rubber particles to make them completely wet, and can be added to the concrete mixture after standing for 20 minutes. Compared with rubber particles that have not been treated in any way, the rubber particles treated by the method of the present invention can greatly improve the strength of rubber concrete, and will not have an adverse effect on the performance of the concrete mixture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a rubber particle modifier for rubber concrete and a preparation method thereof. Background Art

[0002] In recent years, the amount of waste tires has increased significantly with the rapid development of China's automobile industry and the rapid increase in the number of cars owned. Waste tires have strong heat resistance and mechanical resistance, and are difficult to degrade. They will not disappear naturally for decades. They are called "black pollution" and pose a great threat to the environment. Waste tires are a renewable resource. Recycling and reuse can not only save resources and reduce pollution, but also create considerable economic benefits. Rubber concrete is a new type of building material made by recycling waste tire rubber and mixing it into ordinary concrete. However, the disadvantages of rubber concrete are also obvious, that is, the compressive strength is greatly reduced compared with ordinary concrete, which greatly limits the engineering application of rubber concrete. Studies have shown that the main reason for the low compressive strength of rubber concrete is that the bonding strength between rubber particles and cement matrix is ​​much smaller than the bonding strength between aggregates and cement matrix, resulting in reduced concrete strength.

[0003] In order to improve the bonding performance between rubber particles and cement matrix, the following methods are usually adopted:

[0004] (1) Soaking rubber particles in water. For example, in 1993, Eldin and Senonic soaked rubber particles in water and found that the compressive strength of concrete was improved compared with that before treatment.

[0005] (2) Inorganic modification: For example, in 2000, Segre, Joekes and others used NaOH solution to soak rubber powder to improve the strength of rubber concrete.

[0006] (3) Organic modification. For example, in 2010, Li Yue et al. used silane-modified styrene acrylic polymer emulsion X, styrene acrylic polymer emulsion Y, and silane coupling agent KH-550 to modify rubber concrete. They found that rubber aggregate interface modification can significantly improve the flexural impact properties of rubber aggregate concrete, among which silane-modified styrene acrylic emulsion has the best effect.

[0007] Although the above methods have improved the strength of rubber concrete to varying degrees, they all have shortcomings: Specifically, the effect of water washing rubber particles is not obvious; the NaOH solution modification method is cumbersome and has certain risks, and the modification effect is related to the concentration, but the optimal concentration is difficult to determine; and the silane-modified polymer emulsion process is relatively complex and costly. Therefore, a modification method of rubber particles with both high cost performance and excellent performance has practical significance and value for improving the strength of rubber concrete and promoting the application of rubber concrete. Summary of the invention

[0008] Although the current treatment method can improve the bonding performance between rubber particles and cement matrix from a certain perspective, it also has certain defects and problems. The present invention provides a rubber particle modifier for rubber concrete and a preparation method thereof.

[0009] The solution adopted by the present invention to solve the technical problem is: a rubber particle modifier for rubber concrete, comprising the following raw materials in parts by mass: 60 parts of epoxy resin Z44, 2 parts of Tween, 1 part of primer stock solution CS-20, 2 parts of OP-10, 8 parts of polyvinyl alcohol, 6 parts of silane coupling agent KH-570, and 112 parts of 75% ethanol solution.

[0010] The present invention also provides a method for preparing the rubber particle modifier for rubber concrete, comprising the following steps:

[0011] (1) Mix Tween, primer solution CS-20 and OP-10, add to Z44, and stir evenly to form a mixed solution I;

[0012] (2) adding polyvinyl alcohol to the mixed solution I, stirring evenly to form a mixed solution II;

[0013] (3) Add silane coupling agent KH570 to mixed solution II, then add ethanol solution, stir evenly to form mixed solution III, and obtain rubber particle modifier.

[0014] The present invention also provides a method for using the rubber particle modifier for rubber concrete, wherein the rubber particle modifier is sprayed evenly onto the surface of the rubber particles to completely wet them, and the rubber particles are added to the concrete mixture after standing for 20 minutes.

[0015] In the method for using the rubber particle modifier for rubber concrete, the amount of the rubber particle modifier added is 20% of the rubber particles.

[0016] Beneficial effects of the present invention: The rubber particle modifier prepared by the present invention breaks the currently commonly used rubber particle modification method. The rubber particles treated with the rubber particle modifier have two effects: (1) a layer of epoxy adhesive film is wrapped on the surface of the rubber particles, which has a strong bonding effect with the cement matrix; (2) a bivalent chemical bond is grafted on the surface of the rubber particles, in which the organic bond is firmly bonded to the rubber particles, and the inorganic bond at the other end is firmly bonded to the cement matrix. Under the influence of these two effects, the rubber particles can be reliably bonded to the cement matrix, thereby improving the strength of the rubber concrete.

[0017] The rubber modifier of the present invention has a simple preparation process and is easy to use. It will not affect the basic performance of concrete, but can also improve the compressive strength. It has high cost performance and excellent performance, and has practical significance and value for improving the strength of rubber concrete and promoting the application of rubber concrete. DETAILED DESCRIPTION

[0018] In view of the problems and defects of the current rubber concrete modification treatment methods, the present invention provides a rubber particle modifier for rubber concrete and a preparation method thereof. The present invention is further described below in conjunction with embodiments.

[0019] Example 1: This example provides a rubber particle modifier for rubber concrete, which includes the following raw materials in parts by mass: 60 parts of epoxy resin Z44, 2 parts of Tween, 1 part of primer stock solution CS-20, 2 parts of OP-10, 8 parts of polyvinyl alcohol, 6 parts of silane coupling agent KH-570, and 112 parts of 75% ethanol solution.

[0020] The base coating solution CS-20 includes water-soluble epoxy resin (>90%), acrylic emulsion (<10%), formaldehyde (<5%) and water.

[0021] The preparation process of the rubber particle modifier comprises the following steps:

[0022] (1) Mix Tween, primer solution CS-20 and OP-10, add to Z44, and stir evenly to form a mixed solution I;

[0023] (2) Add polyvinyl alcohol to mixed solution I and stir to form mixed solution II

[0024] (3) Add silane coupling agent KH570 to mixed solution II, then add ethanol solution, and stir evenly to form mixed solution III, i.e., rubber particle modifier.

[0025] The prepared rubber particle modifier is used to modify the rubber particles, and the method of use is as follows:

[0026] Take 20% of the rubber particle mass of the rubber particle modifier and spray it evenly on the surface of the rubber particles to make them completely wet. After standing for 20 minutes, the rubber particles can be mixed into the concrete mixture.

[0027] In order to verify the application effect of the rubber particle modifier prepared in Example 1 of the present invention in rubber concrete, the present invention also provides the following comparative examples for comparison and explanation, wherein the materials used are all from the same batch of raw materials, cement is composite silicate cement, strength grade is 42.5; sand is river sand, fineness modulus is 3.2; gravel is limestone crushed stone; rubber particle size is 2-3mm. The ordinary concrete mix ratio mentioned below is: water: cement: sand: gravel = 21: 34: 66: 119; rubber concrete (rubber particle modified and unmodified) mix ratio is: water: cement: sand: rubber particle: gravel = 21: 34: 60: 3: 119

[0028] Comparative Example 1: This comparative example uses ordinary concrete as a comparative example.

[0029] Comparative Example 2: In this comparative example, ordinary rubber concrete was prepared using unmodified rubber particles.

[0030] Comparative Example 3: In this comparative example, the rubber particles were treated by soaking them in water, and then rubber concrete was prepared using the rubber particles.

[0031] The treatment method is: wash the rubber particles with a particle size of 2-3 mm with clean water 2-3 times, place them in a cool place to dry, and then prepare rubber concrete according to the ratio.

[0032] Comparative Example 4: In this comparative example, rubber particles are modified by inorganic modification, and then rubber concrete is prepared therefrom.

[0033] The treatment method is: modify the rubber particles with a 20% NaOH aqueous solution. The treatment method is: prepare a 20% NaOH aqueous solution, soak rubber particles with a particle size of 2 to 3 mm in the NaOH aqueous solution for 24 hours, then take out the rubber particles and wash them with clean water 2 to 3 times until the pH is 7, and then dry them to prepare rubber concrete.

[0034] Comparative Example 5: In this comparative example, rubber particles are modified by organic modification, and then rubber concrete is prepared using the modified rubber particles. The reagents used are: 20% NaOH aqueous solution and liquid silane coupling agent KH570, wherein KH570 is a KH570 solution obtained by diluting 1% of the mass of the rubber particles with an ethanol solution.

[0035] The treatment method is: first soak the rubber particles in NaOH aqueous solution for 24 hours, then wash the rubber particles with water once, and then fully moisten the rubber particles with a particle size of 2 to 3 mm with KH570 solution, and prepare rubber concrete after drying.

[0036] Then, the slump and compressive strength of the rubber concrete prepared in Example 1 and Comparative Examples 1-5 were measured respectively. The results are shown in Table 1.

[0037] Table 1 Test results of slump and compressive strength of rubber concrete

[0038]

[0039] Note: The decrease in the table is calculated based on comparative example 1; the increase is calculated based on comparative example 2.

[0040] As can be seen from Table 1, the rubber concrete prepared by the rubber particles treated with the rubber particle modifier and modification method of the present invention has little difference in overall concrete slump compared with the rubber concrete prepared by the rubber particles obtained in Comparative Examples 1-5, indicating that the modified rubber particles of the present invention have little effect on the working performance of the concrete, but significantly improve the compressive strength.

[0041] The above description is only a preferred embodiment of the present invention and does not limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A rubber particle modifier for rubber concrete, characterized in that: The raw materials include the following parts by weight: 60 parts of epoxy resin Z44, 2 parts of Tween, 1 part of primer stock solution CS-20, 2 parts of OP-10, 8 parts of polyvinyl alcohol, 6 parts of silane coupling agent KH-570, and 112 parts of 75% ethanol solution; The primer solution CS-20 includes water-soluble epoxy resin, acrylic emulsion, formaldehyde and water.

2. The method for preparing the rubber particle modifier for rubber concrete according to claim 1, characterized in that: The following steps are involved: Mix Tween, primer stock solution CS-20 and OP-10, add to Z44, and stir evenly to form mixed solution Ⅰ; Add polyvinyl alcohol to mixed solution I, stirring evenly to form mixed solution II; The silane coupling agent KH570 is added to the mixed solution II, and then the ethanol solution is added and stirred evenly to form a mixed solution III, thereby obtaining a rubber particle modifier.

3. The method for using the rubber particle modifier for rubber concrete according to claim 1, characterized in that: Take the rubber particle modifier and spray it evenly onto the surface of the rubber particles to make them completely wet. After standing for 20 minutes, the rubber particles can be mixed into the concrete mixture.

4. The method for using the rubber particle modifier for rubber concrete according to claim 3, characterized in that: The amount of rubber particle modifier added is 20% of the rubber particles.

Citation Information

Patent Citations

  • Surface modification method of rubber aggregate for high-fluidity cement-based material

    CN101935175A

  • High-strength wear-resistant modified natural rubber and preparation method thereof

    CN111138725A

  • Modified EPS particles, modification method thereof, concrete containing modified EPS particles and preparation method of concrete

    CN114315412A

  • Cement concrete added with modified waste tire rubber powder as well as preparation method and application of cement concrete