A method for synthesizing low molecular weight polystyrene
Through free radical polymerization of zinc-based or iron-based catalysts and benzyl or allyl halogenated hydrocarbons, the problems of high water and oxygen removal requirements, high cost and safety risks in the synthesis process of low molecular weight polystyrene in the existing technology are solved. , achieving efficient synthesis and excellent flame retardant properties of low molecular weight polystyrene.
Patent Information
- Application Number
- CN202310369429.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-04-07
AI Technical Summary
Existing low molecular weight polystyrene synthesis methods have strict water and oxygen removal requirements, high process costs and safety risks, and it is difficult to produce low molecular weight materials through traditional free radical polymerization, resulting in poor flame retardant properties.
Zinc or iron catalysts and benzyl or allyl halogenated hydrocarbons are used as free radical initiators to perform traditional free radical polymerization to synthesize low molecular weight polystyrene. The reaction temperature is 40 to 140°C, and strict water removal is not required. Oxygen, the process is simple, the process cost is low, and the catalyst used is safer.
It achieves efficient synthesis of low molecular weight polystyrene with narrow molecular weight distribution, reduces process costs, improves safety, and produces flame retardants with excellent performance.
Smart Images

Figure BDA0004168112500000021 
Figure BDA0004168112500000022 
Figure BDA0004168112500000023
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer flame retardant synthesis, in particular to a method for synthesizing low molecular weight polystyrene. Background Art
[0002] Low molecular weight polystyrene is the main raw material for synthesizing high molecular weight brominated flame retardants. High molecular weight brominated flame retardants are the most widely used organic flame retardants in the world. The biggest problem currently faced by this flame retardant is its poor compatibility with the flame-retardant substrate. It is easy to precipitate frost, resulting in a decrease in flame retardancy and deterioration of the mechanical properties of the material, and easy breakage or welds. The main reason for the poor compatibility is the poor adhesion between the flame retardant and the polymer material and the high interface energy. According to thermodynamics, the compatibility of two liquids when mixed is measured by Gibbs free energy, as shown in formula (1):
[0003] ΔG=ΔH-TΔS Formula (1)
[0004] ΔG>0, incompatible; ΔG<0, compatible. Analyzing this formula, when two liquids are mixed, the mixing heat is endothermic, so the enthalpy change ΔH is positive. If the entropy increases, the entropy change ΔS increases, and only then can ΔG<0. The flame-retarded substrate has a higher order, so the entropy increase is smaller. Therefore, only by reducing the molecular weight of the flame retardant and increasing its entropy can the compatibility of the two be increased. Therefore, the synthesis of low molecular weight polystyrene is of great significance to the development of brominated flame retardants.
[0005] The synthesis methods of low molecular weight polystyrene currently mainly include anionic polymerization, atom transfer radical polymerization (ATRP) and traditional free radical polymerization. These methods have high requirements for raw material purity and process flow. For example, CN101240046A uses ATRP to prepare low polystyrene, but the process has high requirements for reaction conditions, and requires the use of a vacuum pump and additional dehydrating agents to remove water and oxygen, which has high requirements for the reaction device and complex process; and the low-priced metal catalyst required is not easy to store, resulting in high process costs. CN109415458A uses anionic polymerization to synthesize low polystyrene, and uses organic lithium reagents in this process. The properties of organic lithium reagents are extremely unstable and easily cause accidents, so this process has a large safety risk. Traditional free radical polymerization can only produce medium molecular weight polystyrene (weight average molecular weight is about 40,000 to 80,000 Daltons), and the flame retardant prepared with this material has poor performance, so traditional free radical polymerization is rarely used for the synthesis of low molecular weight polystyrene. Summary of the invention
[0006] The purpose of the present invention is to provide a method for synthesizing low molecular weight polystyrene. The reaction process of the present invention does not require strict water removal and oxygen removal, has low requirements on the reaction device, is simple in process, and has low process cost; and does not use an organic lithium catalyst, so the safety is higher.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for synthesizing low molecular weight polystyrene, comprising the following steps:
[0009] Mixing monomers, free radical initiators and catalysts to carry out polymerization reaction to obtain low molecular weight polystyrene; the polymerization reaction temperature is 40 to 140°C;
[0010] The monomer is styrene or substituted styrene;
[0011] The free radical initiator is a benzyl halogenated hydrocarbon or an allyl halogenated hydrocarbon;
[0012] The catalyst is a zinc-based catalyst or an iron-based catalyst; the zinc-based catalyst is one or more of zinc oxide, zinc salt and zinc complex; the iron-based catalyst is one or more of iron oxide, iron salt and iron complex.
[0013] Preferably, the benzyl halogenated hydrocarbon has a structure shown in Formula 1:
[0014]
[0015] In formula 1, X = Br, I or Cl;
[0016] R, R1, R2, R3, R4 and R5 are independently selected from one of -H, -CH3, -Br, -I, -Cl and -OCH3.
[0017] Preferably, the allyl halide has a structure shown in Formula 2:
[0018]
[0019] In formula 2, X = Br, I or Cl;
[0020] R1, R2 and R3 are independently selected from one of -H, -CH3, -Br, -I, -Cl and -OCH3.
[0021] Preferably, the zinc oxide includes zinc oxide; the zinc salt includes one or more of zinc bromide, zinc sulfate and zinc oxalate; the zinc complex includes one or more of zinc acetylacetonate, sodium zinc ethylenediaminetetraacetate and the zinc complex shown in Formula 3;
[0022]
[0023] The iron oxide includes iron oxide; the iron salt includes one or more of ferric bromide, ferric nitrate and iron sulfide; the iron complex includes one or more of ferric triacetylacetonate, potassium hexacyanoferrate and ferric thiocyanate.
[0024] Preferably, the mass ratio of the monomer to the free radical initiator is (20-20000): (1-100).
[0025] Preferably, the mass ratio of the monomer to the catalyst is (1000-1000000): (1-30).
[0026] Preferably, the polymerization reaction time is 0.1 to 120 hours.
[0027] Preferably, after the polymerization reaction, the obtained reaction product is further subjected to post-treatment; the post-treatment comprises: dissolving the reaction product in a good solvent for polystyrene, filtering to remove insoluble solid impurities, concentrating the obtained filtrate, pouring the concentrated solution into a poor solvent for polystyrene for sedimentation, filtering, and drying the obtained solid to obtain low molecular weight polystyrene.
[0028] Preferably, the polymerization reaction further comprises replacing the air in the reaction container with nitrogen before the polymerization reaction.
[0029] Preferably, the weight average molecular weight of the low molecular weight polystyrene is between 2000 and 10000, and the molecular weight distribution is less than 2.
[0030] The invention provides a method for synthesizing low molecular weight polystyrene, comprising the following steps: mixing a monomer, a free radical initiator and a catalyst, and performing a polymerization reaction to obtain the low molecular weight polystyrene; the polymerization reaction temperature is 40-140 DEG C; the monomer is styrene or substituted styrene; the free radical initiator is a benzyl halogenated hydrocarbon or an allyl halogenated hydrocarbon; the catalyst is a zinc catalyst or an iron catalyst; the zinc catalyst is one or more of zinc oxide, zinc salt and zinc complex; the iron catalyst is one or more of iron oxide, iron salt and iron complex.
[0031] The invention uses a zinc or iron catalyst system and uses benzyl or allyl halogenated hydrocarbon as a free radical initiator to induce styrene to undergo traditional free radical polymerization to synthesize low molecular weight polystyrene. The weight average molecular weight of the polystyrene synthesized by the invention is between 2000 and 10000, and the molecular weight distribution is narrow, less than 2.
[0032] The advantages of the present invention are: 1. The reaction process does not require strict water and oxygen removal, has low requirements for the reaction device, is simple in process, and has low process cost. 2. The zinc or iron catalyst system used is safer and more stable than the traditional organic lithium catalyst, and has less harm to the human body and the environment. 3. The benzyl or allyl halogenated hydrocarbon used as the free radical initiator has no explosion risk and is safer than the traditional free radical initiators such as benzoyl peroxide. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 to Figure 14 The gel permeation chromatography (GPC) spectra of Examples 1 to 14 are shown in order. DETAILED DESCRIPTION
[0034] The present invention provides a method for synthesizing low molecular weight polystyrene, comprising the following steps:
[0035] Mixing monomers, free radical initiators and catalysts to carry out polymerization reaction to obtain low molecular weight polystyrene; the polymerization reaction temperature is 40 to 140°C;
[0036] The monomer is styrene or substituted styrene;
[0037] The free radical initiator is a benzyl halogenated hydrocarbon or an allyl halogenated hydrocarbon;
[0038] The catalyst is a zinc-based catalyst or an iron-based catalyst; the zinc-based catalyst is one or more of zinc oxide, zinc salt and zinc complex; the iron-based catalyst is one or more of iron oxide, iron salt and iron complex.
[0039] In the present invention, unless otherwise specified, the raw materials used are commercially available products well known in the art.
[0040] In the present invention, the monomer is styrene or substituted styrene. The present invention has no special requirements on the type of the substituted styrene, and any styrene with a substituent on the benzene ring known in the art can be used, specifically, 4-bromostyrene, 1,4-dibromostyrene, 1,2,3-tribromostyrene, 2,3,4-tribromostyrene, 1,2,4-tribromostyrene.
[0041] In the present invention, the free radical initiator is a benzyl halogenated hydrocarbon or an allyl halogenated hydrocarbon; the benzyl halogenated hydrocarbon preferably has a structure shown in Formula 1:
[0042]
[0043] In formula 1, X = Br, I or Cl;
[0044] R, R1, R2, R3, R4 and R5 are independently selected from one of -H, -CH3, -Br, -I, Cl and -OCH3.
[0045] In the present invention, the benzyl halogenated hydrocarbon is more preferably 1-bromoethylbenzene.
[0046] In the present invention, the allyl halide preferably has a structure shown in Formula 2:
[0047]
[0048] In formula 2, X = Br, I or Cl;
[0049] R1, R2 and R3 are independently selected from one of -H, -CH3, -Br, -I, -Cl and -OCH3.
[0050] The benzyl or allyl halogenated hydrocarbon used in the present invention as a free radical initiator has no explosion risk and is safer than traditional free radical initiators such as benzoyl peroxide.
[0051] In the present invention, the catalyst is a zinc catalyst or an iron catalyst; the zinc catalyst is one or more of zinc oxide, zinc salt and zinc complex; the iron catalyst is one or more of iron oxide, iron salt and iron complex. In the present invention, the zinc oxide preferably includes zinc oxide; the zinc salt preferably includes one or more of zinc bromide, zinc sulfate and zinc oxalate; the zinc complex preferably includes zinc acetylacetonate, sodium zinc ethylenediaminetetraacetate and
[0052] One or more of the zinc complexes shown in Formula 3.
[0053]
[0054] In the present invention, the iron oxide preferably includes iron oxide; the iron salt preferably includes one or more of ferric bromide, ferric nitrate and iron sulfide; the iron complex preferably includes one or more of ferric triacetylacetonate, potassium hexacyanoferrate and ferric thiocyanate. The zinc or iron catalytic system used in the present invention is safer and more stable than the traditional organic lithium catalyst, and has less harm to the human body and the environment.
[0055] In the present invention, the mass ratio of the monomer to the free radical initiator is preferably (20-20000):(1-100), more preferably 200:1.
[0056] In the present invention, the mass ratio of the monomer to the catalyst is preferably (1000-1000000):(1-30), more preferably 100000:9.
[0057] The present invention has no special requirements for the process of mixing the monomer, free radical initiator and catalyst. Any method known in the art for uniformly mixing the raw materials can be used, such as uniform stirring.
[0058] Before the polymerization reaction, the present invention preferably replaces the air in the reaction container with nitrogen. In the present invention, the flow rate of nitrogen is preferably 20 to 60 mL / min, and the time is preferably 30 to 60 min.
[0059] In the present invention, the polymerization reaction temperature is 40 to 140°C, preferably 50 to 120°C, and more preferably 65 to 100°C; the polymerization reaction time is preferably 0.1 to 120 hours, more preferably 5 to 100 hours, further preferably 10 to 50 hours, and most preferably 24 to 36 hours.
[0060] After the polymerization reaction is completed, the present invention does not perform any post-treatment to directly obtain low molecular weight polystyrene or performs post-treatment on the obtained reaction product to obtain low molecular weight polystyrene with higher purity.
[0061] When post-treatment is performed, the post-treatment preferably includes: dissolving the reaction product in a good solvent for polystyrene, filtering to remove insoluble solid impurities, concentrating the obtained filtrate, pouring the concentrated solution into a poor solvent for polystyrene for sedimentation, filtering, and drying the obtained solid to obtain low molecular weight polystyrene. In the present invention, the good solvent preferably includes tetrahydrofuran or chloroform; the poor solvent preferably includes methanol, ether, n-hexane, n-heptane or n-octane. The present invention can remove metal ion catalysts through post-treatment.
[0062] In the present invention, the weight average molecular weight of the low molecular weight polystyrene is preferably between 2000 and 10000, and the molecular weight distribution is preferably less than 2, which has the advantages of low molecular weight and narrow molecular weight distribution range.
[0063] The synthesis method of low molecular weight polystyrene provided by the present invention is described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0064] Example 1
[0065] 1 mg of zinc oxide, 0.01 g of 1-bromoethylbenzene and 1 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 65°C for 48 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 3 mL at 50°C, 30 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 3122 and the dispersion coefficient was 1.6 (see GPC). Figure 1 ).
[0066] Example 2
[0067] 1 mg of zinc oxide, 0.05 g of 1-bromoethylbenzene and 1 g of commercially available 4-bromostyrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 65°C for 48 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 3 mL at 50°C, 30 mL of methanol was added, and the light yellow precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight poly-4-bromostyrene. The weight average molecular weight was 9675 and the dispersion coefficient was 1.5 (see GPC). Figure 2 ).
[0068] Example 3
[0069] 1 mg of zinc oxide, 0.01 g of 1-(bromomethyl)benzene and 1 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 65°C for 48 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 3 mL at 50°C, 30 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 2816 and the dispersion coefficient was 1.7 (see GPC). Figure 3 ).
[0070] Example 4
[0071] 1 mg of zinc bromide, 0.01 g of 1-bromoethylbenzene and 1 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 65°C for 48 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 3 mL at 50°C, 30 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 3990 and the dispersion coefficient was 1.5 (see GPC). Figure 4 ).
[0072] Example 5
[0073] 9 mg of zinc bromide, 0.05 g of 1-bromoethylbenzene and 10 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 50 minutes, the polymerization reaction was carried out at 65°C for 24 hours. After the reaction was completed, 40 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 20 mL at 50°C, 200 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 5699 and the dispersion coefficient was 1.3 (see GPC). Figure 5 ).
[0074] Example 6
[0075] 1 mg of zinc oxide, 0.01 g of 1-bromoethylbenzene and 1 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 140°C for 2 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 3 mL at 50°C, 30 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 2728 and the dispersion coefficient was 1.7 (see GPC). Figure 6 ).
[0076] Example 7
[0077] 9 mg of zinc bromide, 0.05 g of 1-bromoethylbenzene and 10 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 50 minutes, the polymerization reaction was carried out at 65°C for 24 hours. After the reaction was completed, 40 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were removed by filtration. After the collected filtrate was concentrated to 10 mL at 50°C, 200 mL of n-hexane was added, and the milky white precipitate produced was collected by filtration and centrifugation. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 7462 and the dispersion coefficient was 2.6 (see GPC). Figure 7 ).
[0078] Example 8
[0079] 9 mg of zinc acetylacetonate, 0.05 g of 1-bromoethylbenzene and 10 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 50 minutes, the polymerization reaction was carried out at 65°C for 24 hours. After the reaction was completed, 40 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 20 mL at 50°C, 200 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 8216 and the dispersion coefficient was 1.3 (see GPC). Figure 8 ).
[0080] Example 9
[0081] The preparation method of the 22-ring Robson-type ligand binuclear zinc catalyst refers to Inorg.Chem.44,147–157 (2005) and Aust.J.Chem.,23,2225–2236 (1970). The specific steps are as follows: In a 25 mL round-bottom flask, Zn(NO3)2·6H2O (0.446 g, 1.5 mmol) is dissolved in 5 mL of methanol. A methanol solution of 1,3-diaminopropane (0.111 g, 0.75 M, 2 mL) and 2-hydroxy-5-methylisophthalaldehyde (0.246 g, 0.2 M, 7.5 mL) is added to the flask and stirred to form a clear solution. After standing at room temperature for two days, the crystallized yellow plate-like crystals are collected. After vacuum drying at room temperature, the 22-ring Robson-type ligand binuclear zinc catalyst is obtained.
[0082] 15 mg of a homemade 22-ring Robson-type ligand binuclear zinc catalyst (structure see formula 3), 0.05 g of 1-bromoethylbenzene and 10 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 50 minutes, the polymerization reaction was carried out at 65°C for 24 hours. After the reaction was completed, 40 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 20 mL at 50°C, 200 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 9640 and the dispersion coefficient was 1.8 (see Fig. 9 ).
[0083]
[0084] Example 10
[0085] 1 mg zinc oxide, 0.01 g 1-bromoethylbenzene and 1 g commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 85°C for 48 hours. After the reaction was completed, the low molecular weight polystyrene solid obtained by the reaction was dissolved in 10 mL tetrahydrofuran, and then the weight average molecular weight of the obtained low molecular weight polystyrene solid was directly measured by gel permeation chromatography (GPC) without post-treatment steps, and the dispersion coefficient was 1.6 (see Fig.10 ).
[0086] Embodiment 11
[0087] 0.3 mg of iron oxide, 0.01 g of 1-bromoethylbenzene and 1 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 50°C for 48 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 3 mL, 30 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 2927 and the dispersion coefficient was 1.5 (see GPC). Fig.11 ).
[0088] Example 12
[0089] 0.3 mg of ferric nitrate, 0.01 g of 1-bromoethylbenzene and 1 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 50°C for 48 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 3 mL, 30 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 3215 and the dispersion coefficient was 1.6 (see GPC). Fig.12 ).
[0090] Example 13
[0091] 1 mg of zinc oxide, 0.01 g of 1-chloroethylbenzene and 1 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 65°C for 48 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were filtered out. After the collected filtrate was concentrated to 3 mL at 50°C, 30 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 5487 and the dispersion coefficient was 1.7 (see GPC). Fig.13 ).
[0092] Embodiment 14
[0093] 1 mg of zinc oxide, 0.005 g of 3-iodo-1-propylene and 1 g of commercially available styrene were added to the reactor and stirred at a uniform speed. After nitrogen was introduced at a flow rate of 30 mL / min to replace the air in the reactor for 30 minutes, the polymerization reaction was carried out at 45°C for 72 hours. After the reaction was completed, 10 mL of tetrahydrofuran was used to dissolve the solid obtained by the reaction, and then the undissolved solid impurities were removed by filtration. After the collected filtrate was concentrated to 3 mL at 50°C, 30 mL of methanol was added, and the white precipitate produced was collected by suction filtration. After drying to constant weight, it was low molecular weight polystyrene. The weight average molecular weight was 6544 and the dispersion coefficient was 1.8 (see GPC). Fig.14 ).
[0094] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for synthesizing low molecular weight polystyrene, It is characterized in that The following steps are involved: Mixing monomers, free radical initiators and catalysts to carry out polymerization reaction to obtain low molecular weight polystyrene; the polymerization reaction temperature is 40 to 140°C; The monomer is styrene or substituted styrene; The free radical initiator is 3-iodo-1-propylene; The catalyst is a zinc-based catalyst or an iron-based catalyst; The zinc catalyst is zinc oxide, zinc bromide, zinc acetylacetonate or a zinc complex as shown in Formula 3; The iron-based catalyst is iron oxide or iron nitrate.
2. The synthesis method according to claim 1, It is characterized in that The mass ratio of the monomer to the free radical initiator is (20-20000): (1-100).
3. The synthesis method according to claim 1, It is characterized in that The mass ratio of the monomer to the catalyst is (1000-1000000): (1-30).
4. The synthesis method according to claim 1, It is characterized in that The polymerization reaction time is 0.1 to 120 hours.
5. The synthesis method according to claim 1 or 4, It is characterized in that After the polymerization reaction, the obtained reaction product is subjected to post-treatment; the post-treatment includes: dissolving the reaction product in a good solvent for polystyrene, filtering to remove insoluble solid impurities, concentrating the obtained filtrate, pouring the concentrated solution into a poor solvent for polystyrene for sedimentation, filtering, and drying the obtained solid to obtain low molecular weight polystyrene.
6. The synthesis method according to claim 1 or 4, It is characterized in that The polymerization reaction also includes replacing the air in the reaction container with nitrogen before the polymerization reaction.
7. The synthesis method according to claim 1, It is characterized in that The weight average molecular weight of the low molecular weight polystyrene is between 2000 and 10000, and the molecular weight distribution is less than 2.
Citation Information
Patent Citations
Method for preparing low molecular weight narrow distribution brominated polystyrene by active / controllable polymerization
CN101240046A
Process and catalyst for hydrogen mediated saline hydride initiated aniconic chain transfer polymerization
CN109415458A
Toxic ligand free electrochemistry regulated atom transfer radical polymerization method
CN106749778A
Atom transfer free radical polymerization method regulated and controlled by inorganic metal salt
CN108546311A
Manufacturing method of narrow molecular weight distributed hydroxystyrene polymer
JP2003183314A