A nanoporous zirconium oxide adsorbent and preparation method thereof

By using nanoporous zirconia adsorbent under normal pressure, the problems of high carbon dioxide capture cost and complicated process in the existing technology are solved, efficient adsorption and simplified process flow are achieved, and the performance and stability of the adsorbent are improved.

CN116550276BActive Publication Date: 2024-10-29TAIYUAN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310656731.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-05
Publication Date
2024-10-29
Estimated Expiration
2043-06-05

AI Technical Summary

Technical Problem

The existing technology is difficult to efficiently capture carbon dioxide under normal pressure, and the amine loading process is complex, which increases costs and process steps.

Method used

Using nanoporous zirconia adsorbent, it is prepared by reacting with cetyltrimethylammonium bromide and organic zirconium source in an ethanol aqueous solution with pH=5~5.5 to form a wet gel and then calcined at high temperature to form a high specific surface area. and zirconia adsorbent materials with uniform pore sizes.

Benefits of technology

It achieves efficient adsorption of carbon dioxide under normal pressure, reduces capture costs, simplifies the process, avoids the amine loading link, and improves the uniformity and dispersion of the adsorbent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116550276B_ABST
    Figure CN116550276B_ABST
Patent Text Reader

Abstract

The present invention relates to a nanoporous zirconium oxide adsorbent, which is a zirconium oxide adsorbent prepared by mixing an organic zirconium source and a cationic template agent, hexadecyltrimethylammonium bromide, in an ethanol aqueous solution with a long-chain aliphatic dicarboxylic acid, dodecanedioic acid, as a dispersant, self-assembling to form a zirconium-containing wet gel through solvent volatilization, and high-temperature calcination. The nanoporous zirconium oxide adsorbent prepared by the present invention has a high specific surface area, does not load amine substances, and has a good selective adsorption effect on carbon dioxide under normal pressure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of gas capture, and relates to an adsorbent for capturing carbon dioxide, and in particular to a zirconium oxide adsorbent for adsorbing carbon dioxide under normal pressure. Background Art

[0002] The global warming and climate change issues caused by the massive emission of carbon dioxide (CO2) greenhouse gas have become the focus of global attention. Carrying out research on CO2 capture and storage technology is one of the important ways to reduce greenhouse gas CO2 emissions and protect the environment.

[0003] Coal-fired power plants are the main stationary source of CO2 emissions. The CO2 content emitted from their flue gases is usually between 3% and 30% (volume fraction). Therefore, it is necessary to separate CO2 from their flue gases, concentrate it into CO2 gas with higher purity, and then transport it to a specific location for long-term storage through pipelines and other means.

[0004] At present, the separation and recovery of CO2 in flue gas is mainly based on chemical adsorption of amine-based solid adsorbents, and the adsorption operation usually needs to be carried out at a pressure of 0.1 to 0.17 MPa. If CO2 can be directly recovered at normal pressure, the cost of capturing CO2 can be saved directly from the source.

[0005] Sohail et al. (Adsorption behavior of tetraethylenepentamine functionalizedSi-MCM-41 for CO2 adsorption[J]. Chemical Engineering Research and Design, 2017, 122: 34-42.) modified Si-MCM-41 with tetraethylenepentamine (TEPA) to prepare a solid amine adsorbent. The results showed that when the TEPA loading was 50wt%, the adsorbent showed a maximum CO2 adsorption capacity of 1.6mmol / g under adsorption conditions of normal pressure and 75℃.

[0006] Recently, Zhao Peiyu et al. (Preparation of amine functional adsorbents and their carbon dioxide adsorption performance [D]. Taiyuan University of Technology, 2020, 35-42.) reported that an adsorbent with good thermal stability was prepared by loading TEPA on the surface of a porous silica carrier. The study found that when the TEPA loading reached 60wt%, the maximum CO2 adsorption capacity obtained by normal pressure adsorption performance test at 75°C was 5.01mmol / g.

[0007] Although the solid amine adsorbents reported in the above literature have achieved a certain amount of CO2 adsorption effect under certain adsorption conditions, loading the amine substances on the surface of the carrier, on the one hand, increases the preparation process steps, and on the other hand, according to a large number of current studies, the structural characteristics of the carrier largely determine the loading effect of the amine and its adsorption effect on CO2. Summary of the invention

[0008] The object of the present invention is to provide a nanoporous zirconia adsorbent and a preparation method thereof, which can have a high CO2 adsorption capacity at normal pressure without the need to load amines and other modifying substances.

[0009] The nanoporous zirconium oxide adsorbent of the present invention is a zirconium oxide adsorbent material prepared by high-temperature calcination using a mixed solution of a long-chain aliphatic dicarboxylic acid dodecanedioic acid as a dispersant and a cationic template agent hexadecyltrimethylammonium bromide in an ethanol aqueous solution at a weak acid condition of pH=5-5.5, adding an organic zirconium source to carry out solvent volatilization and self-assembly to form a zirconium-containing wet gel.

[0010] Specifically, the organic zirconium source is any one of zirconium n-butoxide, zirconium n-propoxide or zirconium isopropoxide.

[0011] Furthermore, the present invention further provides a specific preparation method of the nanoporous zirconia adsorbent, comprising the following steps:

[0012] 1) Dissolve dodecanedioic acid in ethanol aqueous solution, adjust the pH value to 5-5.5, and add hexadecyltrimethylammonium bromide to obtain a mixed solution;

[0013] 2) Add an organic zirconium source dropwise to the mixed solution, stir to carry out solvent evaporation self-assembly reaction to obtain a wet gel;

[0014] 3) After the wet gel is dried, the temperature is raised to 550-600° C. and calcined to prepare a nanoporous zirconia adsorbent material.

[0015] Specifically, the molar ratio of the raw materials dodecanedioic acid, hexadecyltrimethylammonium bromide and organic zirconium source is 1:2-2.5:12-15.

[0016] Furthermore, in the ethanol aqueous solution, the volume ratio of ethanol to water is preferably 8-12:1, more preferably 10:1.

[0017] Furthermore, the reaction time for the solvent evaporation self-assembly to obtain the wet gel in the present invention is preferably 20 to 24 hours.

[0018] More preferably, the present invention is to dry the obtained wet gel at 60-65°C.

[0019] Preferably, the calcination time for preparing the nanoporous zirconia adsorbent of the present invention is preferably 4 to 6 hours.

[0020] More preferably, the present invention prepares the nanoporous zirconia adsorbent by heating the material to the calcination temperature at a heating rate of 1 to 5°C / min and then calcining the material at the temperature.

[0021] In the process of preparing the nanoporous zirconia adsorbent, the present invention simultaneously introduces a dicarboxylic acid with a carboxyl group and a cationic template agent, hexadecyltrimethylammonium bromide, and utilizes the interaction between the polar base group contained in the head of the alkyl chain of the template agent and the carboxyl group to form a new ultra-large molecular substance with a larger spatial structure, thereby effectively preventing a large amount of agglomeration of zirconia particles, and preparing a nanoporous zirconia adsorbent with a high specific surface area, uniform and controllable pore size, and a high adsorption amount.

[0022] The nanoporous zirconia adsorbent prepared by the present invention has the advantages of high specific surface area and uniform pore size distribution, and its specific surface area is as high as 106m 2 / g, and the adsorbent particles are not agglomerated, and maintain a highly uniform dispersion state.

[0023] The present invention utilizes the above-prepared nanoporous zirconia adsorbent with excellent structural characteristics directly as a CO2 adsorption material, and has the following technical effects compared with the prior art:

[0024] 1. At present, the separation and recovery of CO2 in flue gas is mainly based on chemical adsorption of modified solid adsorbents. The nanoporous zirconium oxide adsorbent of the present invention can be directly used as a CO2 adsorption material without the need to load amine substances, thus reducing the amine loading process steps;

[0025] 2. The current adsorption operating pressure is usually 0.1-0.17 MPa. The nanoporous zirconia adsorbent of the present invention can directly recover CO2 at normal pressure, greatly saving the recovery cost;

[0026] 3. It solves the problems of increased subsequent CO2 capture costs due to the existing high-pressure CO2 adsorption, as well as the complex existing adsorbent loading process and low CO2 adsorption capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is the infrared spectrum of the nanoporous zirconia adsorbent prepared in Example 1.

[0028] Figure 2 This is the XRD diagram of the nanoporous zirconia adsorbent prepared in Example 1.

[0029] Figure 3 This is a SEM image of the nanoporous zirconia adsorbent prepared in Example 1.

[0030] Figure 4 These are the TEM and HRTEM images of the nanoporous zirconia adsorbent prepared in Example 1.

[0031] Figure 5 This is the N2 physical adsorption isotherm diagram of the nanoporous zirconia adsorbent prepared in Example 1.

[0032] Figure 6 This is the pore size distribution diagram of the nanoporous zirconia adsorbent prepared in Example 1. Implementation

[0033] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are only used to more clearly illustrate the technical solution of the present invention so that those skilled in the art can well understand and utilize the present invention, rather than limiting the scope of protection of the present invention.

[0034] The production processes, experimental methods or detection methods involved in the embodiments of the present invention, unless otherwise specified, are all conventional methods in the prior art, and their names and / or abbreviations are all conventional names in the field, and are very clear and definite in the relevant application fields. Those skilled in the art can understand the conventional process steps based on the names and apply the corresponding equipment, and implement them according to conventional conditions or the conditions recommended by the manufacturer.

[0035] The various instruments, equipment, raw materials or reagents used in the embodiments of the present invention are not particularly limited in terms of their sources, and are all conventional products that can be purchased through regular commercial channels, or can be prepared according to conventional methods well known to those skilled in the art. Example

[0036] Example 1

[0037] Weigh 0.16 g (0.7 mmol) of dodecanedioic acid and add it to a mixed solution of 20 ml of anhydrous ethanol and 2 ml of deionized water. Stir at 40°C for 15 min. Adjust the pH of the solution to 5 with aqueous ammonia. Continue stirring at 40°C for 30 min to obtain a colorless transparent solution.

[0038] 0.5 g (1.4 mmol) of hexadecyltrimethylammonium bromide was added to the above solution, and the mixture was stirred at 40°C for 2 h. Then 3.84 g (10.01 mmol) of zirconium n-butoxide was added dropwise, and the mixture was stirred at 40°C for 20 h to obtain a wet gel.

[0039] The wet gel was filtered and washed with anhydrous ethanol for three times to obtain a white precipitate. The precipitate was dried at 65°C for 2 hours to obtain a white powder, which was then heated to 550°C at a rate of 1°C / min and calcined for 5 hours to prepare a nanoporous zirconia adsorbent.

[0040] The prepared adsorbent was pressed into a KBr pellet and characterized by infrared spectroscopy. Figure 1 As shown, 3433cm -1 The obvious absorption peak appears at 1626cm -1 and 1406cm -1 The absorption peaks at 889cm-1 are the vibration peaks of physically adsorbed water in KBr tablets and the bending vibration peaks of -OH in ZrOH; -1 and 527cm -1 All of them are attributed to the Zr-O bond vibration absorption, proving that tetragonal ZrO2 was successfully synthesized.

[0041] Figure 2 In the X-ray diffraction pattern of the adsorbent, obvious tetragonal phase characteristic diffraction peaks corresponding to the ZrO2 crystal planes (011), (110), (020), (202), and (222) appeared near 2θ=30°, 35°, 50°, 60°, and 62°, which were basically consistent with the tetragonal ZrO2 standard card (JCPDS 89-6976), and the diffraction peak intensity was very high, without other impurity diffraction peaks, indicating that pure tetragonal phase structure ZrO2 with good crystallinity was successfully prepared.

[0042] Furthermore, according to Figure 3 Scanning electron microscope (SEM) images of the provided adsorbent material in different fields of view show that the adsorbent material not only presents very uniform spherical nanoparticles, but also exhibits good pore characteristics.

[0043] Figure 4 Transmission electron microscopy (TEM) and high-magnification transmission electron microscopy (HRTEM) images of the adsorbent material under different fields of view are further presented, from which obvious lattice fringes can be clearly seen, indicating that the synthesized adsorbent material is a zirconium oxide nanocrystalline material.

[0044] from Figure 3 and Figure 4 It can also be seen that the spherical nanoparticles undergo soft agglomeration, and small spherical particles accumulate to form large spherical particles with higher porosity, which is conducive to loading and adsorption.

[0045] Figure 5The physical adsorption-desorption isotherm of the above-mentioned nanoporous zirconia adsorbent is given. It can be clearly seen from the figure that the isotherm belongs to the IV type adsorption isotherm and the H2 type hysteresis loop, which confirms its spherical structure. The adsorption curve and the desorption curve accompanied by a uniform hysteresis loop prove the successful synthesis of the mesoporous material and the uniform nanoparticle morphology. The capillary condensation phenomenon occurring above the relative pressure of 0.4 also proves the existence of larger mesoporous channels. Secondly, the continuous adsorption of nitrogen at a relative pressure close to 1.0 shows that macropores as secondary pores also exist in the material.

[0046] Furthermore, according to Figure 6 It can also be seen from the adsorbent pore size distribution diagram that the adsorbent material exhibits an average pore size of 3.5 nm and presents a highly uniform pore size distribution characteristic.

[0047] Example 2

[0048] Weigh 0.17 g (0.74 mmol) of dodecanedioic acid and add it to a mixed solution of 20 ml of anhydrous ethanol and 2 ml of deionized water. Stir at 42 °C for 15 min, adjust the pH of the solution to 5.5 with ammonia water, and continue stirring at 42 °C for 30 min to obtain a colorless transparent solution.

[0049] 0.55 g (1.5 mmol) of hexadecyltrimethylammonium bromide was added to the above solution, and the mixture was stirred at 42° C. for 2.5 h. Then, 4 g (10.4 mmol) of zirconium n-butoxide was added dropwise, and the mixture was stirred at 42° C. for 21 h to obtain a wet gel.

[0050] The wet gel was filtered and washed with anhydrous ethanol for three times to obtain a white precipitate. The precipitate was dried at 60°C for 2 hours to obtain a white powder, which was then heated to 560°C at a rate of 2°C / min and calcined for 5 hours to prepare a nanoporous zirconia adsorbent.

[0051] Example 3

[0052] Weigh 0.184 g (0.8 mmol) of dodecanedioic acid and add it to a mixed solution of 20 ml of anhydrous ethanol and 2 ml of deionized water. Stir at 38°C for 20 min, adjust the pH of the solution to 5 with ammonia water, and continue stirring at 38°C for 35 min to obtain a colorless transparent solution.

[0053] 0.66 g (1.8 mmol) of hexadecyltrimethylammonium bromide was added to the above solution, and the mixture was stirred at 38° C. for 2.5 h. Then, 4.22 g (11 mmol) of zirconium n-butoxide was added dropwise, and the mixture was stirred at 38° C. for 22 h to obtain a wet gel.

[0054] The wet gel was filtered and washed with anhydrous ethanol for three times to obtain a white precipitate. The precipitate was dried at 65°C for 2.5 hours to obtain a white powder, which was then heated to 555°C at a rate of 1.5°C / min and calcined for 5.5 hours to prepare a nanoporous zirconia adsorbent.

[0055] Comparative Example 1

[0056] Weigh 0.14 g (0.7 mmol) of sebacic acid and add it to a mixed solution of 20 ml of anhydrous ethanol and 2 ml of deionized water. Stir at 40°C for 15 min. Adjust the pH of the solution to 5 with aqueous ammonia and continue stirring at 40°C for 30 min to obtain a colorless transparent solution.

[0057] 0.5 g (1.4 mmol) of hexadecyltrimethylammonium bromide was added to the above solution, and the mixture was stirred at 40°C for 2 h. Then 3.84 g (10.01 mmol) of zirconium n-butoxide was added dropwise, and the mixture was stirred at 40°C for 20 h to obtain a wet gel.

[0058] The wet gel was filtered and washed with anhydrous ethanol for three times to obtain a white precipitate. The precipitate was dried at 65°C for 2 hours to obtain a white powder, which was then heated to 550°C at a rate of 1°C / min and calcined for 5 hours to prepare a nanoporous zirconia adsorbent.

[0059] Comparative Example 2

[0060] Weigh 0.16 g (0.7 mmol) of dodecanedioic acid and add it to a mixed solution of 20 ml of anhydrous ethanol and 2 ml of deionized water. Stir at 40°C for 15 min. Adjust the pH of the solution to 10.5 with aqueous ammonia. Continue stirring at 40°C for 30 min to obtain a colorless transparent solution.

[0061] 0.5 g (1.4 mmol) of hexadecyltrimethylammonium bromide was added to the above solution, and the mixture was stirred at 40°C for 2 h. Then 3.84 g (10.01 mmol) of zirconium n-butoxide was added dropwise, and the mixture was stirred at 40°C for 20 h to obtain a wet gel.

[0062] The wet gel was filtered and washed with anhydrous ethanol for three times to obtain a white precipitate. The precipitate was dried at 65°C for 2 hours to obtain a white powder, which was then heated to 550°C at a rate of 1°C / min and calcined for 5 hours to prepare a nanoporous zirconia adsorbent.

[0063] Comparative Example 3

[0064] Weigh 0.16 g (0.7 mmol) of dodecanedioic acid and add it to a mixed solution of 20 ml of anhydrous ethanol and 2 ml of deionized water. Stir at 40°C for 15 min. Adjust the pH of the solution to 7 with aqueous ammonia. Continue stirring at 40°C for 30 min to obtain a colorless transparent solution.

[0065] 0.5 g (1.4 mmol) of hexadecyltrimethylammonium bromide was added to the above solution, and the mixture was stirred at 40°C for 2 h. Then 3.84 g (10.01 mmol) of zirconium n-butoxide was added dropwise, and the mixture was stirred at 40°C for 20 h to obtain a wet gel.

[0066] The wet gel was filtered and washed with anhydrous ethanol for three times to obtain a white precipitate. The precipitate was dried at 65°C for 2 hours to obtain a white powder, which was then heated to 550°C at a rate of 1°C / min and calcined for 5 hours to prepare a nanoporous zirconia adsorbent.

[0067] The specific surface area of ​​the porous zirconia adsorbent prepared above was measured by physical adsorption instrument and was as high as 106m 2 / g.

[0068] In order to demonstrate the carbon dioxide adsorption performance of the nanoporous zirconia adsorbent prepared by the present invention, the adsorbent materials prepared in the above embodiments and control examples were taken to test the carbon dioxide adsorption performance under normal pressure and 75°C adsorption temperature conditions. The results are shown in Table 1.

[0069]

[0070] The above embodiments of the present invention do not describe all the details in detail, nor limit the present invention to the above embodiments. Various changes, modifications, substitutions and variations made by ordinary technicians in this field without departing from the principles and purpose of the present invention should be included in the protection scope of the present invention.

Claims

1. A nanoporous zirconium oxide adsorbent is a zirconium oxide adsorbent prepared by using a long-chain aliphatic dicarboxylic acid dodecanedioic acid as a dispersant and a cationic template agent hexadecyltrimethylammonium bromide to form a mixed solution in an ethanol aqueous solution at a weak acid condition of pH=5-5.5, adding an organic zirconium source to carry out solvent volatilization and self-assembly to form a zirconium-containing wet gel, and then high-temperature calcination.

2. The nanoporous zirconia adsorbent according to claim 1, characterized in that The organic zirconium source is any one of zirconium n-butoxide, zirconium n-propoxide or zirconium isopropoxide.

3. The method for preparing the nanoporous zirconia adsorbent according to claim 1, comprising: 1) Dissolve dodecanedioic acid in ethanol aqueous solution, adjust the pH value to 5-5.5, and add hexadecyltrimethylammonium bromide to obtain a mixed solution; 2) Add an organic zirconium source dropwise to the mixed solution, stir to carry out solvent evaporation self-assembly reaction to obtain a wet gel; 3) After the wet gel is dried, the temperature is raised to 550-600° C. and calcined to prepare a nanoporous zirconia adsorbent material.

4. The method for preparing the nanoporous zirconia adsorbent according to claim 3, characterized in that The molar ratio of the dodecanedioic acid, hexadecyltrimethylammonium bromide and the organic zirconium source is 1:2-2.5:12-15.

5. The method for preparing the nanoporous zirconia adsorbent according to claim 3, characterized in that The volume ratio of ethanol to water in the ethanol aqueous solution is 8-12:

1.

6. The method for preparing the nanoporous zirconia adsorbent according to claim 3, characterized in that The solvent volatilization self-assembly reaction time is 20 to 24 hours.

7. The method for preparing the nanoporous zirconia adsorbent according to claim 3, characterized in that The wet gel was dried at 60-65°C.

8. The method for preparing the nanoporous zirconia adsorbent according to claim 3, characterized in that The calcination time is 4 to 6 hours.

Citation Information

Patent Citations

  • Carbon dioxide adsorption material in high-temperature flue gas as well as production method and use

    CN101497019A

  • Composite preparation method of submillimeter zirconia ceramic microbeads

    CN112457005A