Catalyst for preparing methacrolein from isobutylene or tert-butyl alcohol, preparation method and application thereof
By using salt or oxide dispersion systems of Mo, Bi, Fe, Co, Ni, V, Mg, Sb, Cs, K and urea hydrolysis technology in the preparation of molybdenum bismuth catalysts, the problem of particle agglomeration in the preparation of molybdenum bismuth catalysts is solved. The activity and selectivity of the catalyst are improved, and the efficient oxidation of isobutene or tert-butanol is achieved.
Patent Information
- Application Number
- CN202210109815.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2042-01-29
AI Technical Summary
During the preparation process, the existing molybdenum bismuth-based catalysts have serious particle agglomeration, which affects the uniformity of components, resulting in low catalyst activity and insufficient selectivity.
During the catalyst preparation process, salts or oxides containing Mo, Bi, Fe, Co, Ni, V, Mg, Sb, Cs, K are added. Through the use of dispersion system and complexing agent, combined with urea, the particles are controlled by slowly hydrolyzing by controlling the granules through the use of dispersion system and complexing agent. Crystallization improves the morphology and uniformity of the catalyst.
The activity and selectivity of the catalyst were significantly improved, the conversion rate of isobutene or tert-butanol was increased by 3.8%, the selectivity of methacreal was increased by 4.9%, and the preparation process was simplified.
Smart Images

Figure BDA0003494764040000081 
Figure BDA0003494764040000082 
Figure BDA0003494764040000083
Abstract
Description
Technical Field
[0001] The invention relates to the field of catalyzing isobutylene or tert-butyl alcohol to prepare methacrolein, and in particular to a catalyst for preparing methacrolein from isobutylene or tert-butyl alcohol, and a preparation method and application thereof. Background Art
[0002] Methyl methacrylate (MMA) is an important organic chemical raw material, mainly used in the production of polymethyl methacrylate (plexiglass), polyvinyl chloride additives and as the second monomer in the production of acrylic fibers. It can also be copolymerized with other vinyl monomers to obtain products of different properties. It is used as resins, adhesives, ion exchange resins, paper polishes, textile printing and dyeing auxiliaries, leather treatment agents, lubricant additives, crude oil depressants, insulating potash materials and plasticizers for plastic emulsions, etc. It has a wide range of uses.
[0003] The wide range of uses and excellent properties of methyl methacrylate have led to rapid development both at home and abroad in recent years. The traditional acetone cyanohydrin process (ACH process) is greatly affected by the transportation or production of acrylonitrile, and the environmental pressure is increasing day by day, so the ACH process is restricted in capacity expansion.
[0004] The isobutylene method (C4 method) is currently a relatively excellent process for producing high value-added MMA. Its raw materials are cheap and pollution-free, and it is a clean route. With the completion of multiple 10 million tons of oil refining and 1 million tons of ethylene projects in my country, as well as the completion of coal chemical MTO, the cracking C4 isobutylene resources are extremely rich, and the advantages of isobutylene oxidation method in producing MMA are gradually reflected.
[0005] The preparation of methacrolein from isobutylene is the first step of this route. The catalyst used for the oxidation of isobutylene to methacrolein is crucial to the development of this route. The catalysts used in this reaction have been studied for many years. The composite oxides of molybdenum, bismuth, iron and cobalt are the most widely used, which has become a consensus among researchers. The catalyst system includes Mo-Bi-P, Mo-Bi-U, Mo-Bi-Fe-Co, Mo-Bi-W-Fe-Co, etc. The most representative Mo-Bi system multi-catalyst composition can be expressed as Mo-Bi-M Ⅱ -M Ⅲ -M Ⅰ -XO, where M Ⅱ It can be Ni 2+ 、Co 2+ Mg 2+ , Mn 2+ , Cu 2+ , Pb 2+ 1-3 of M Ⅲ Fe 3+ Cr 3+ 、Al 3+ ;MⅠ K + 、Na + , Cs + 、Tl + etc.; X is P, B, etc. Among them, Mo is the main component of the catalyst, and its content is relatively large, accounting for about 50% in the catalyst. Bi and other components almost form composite oxides with Mo. Part of the Mo in the catalyst can be replaced by Sb, V, W, Te, etc. Bi is an indispensable component, and the addition amount is small, generally less than 5%. More will damage the activity. The rest is mostly M Ⅱ and M Ⅲ , while M Ⅰ , P, B, etc. are trace components. Ⅲ Mainly Fe 3+ , which can adjust the Fermi level and enhance the redox ability of the catalyst, M Ⅰ 、M Ⅱ The alkali metals and alkaline earth metals in the catalyst can adjust the acidity and alkalinity of the catalyst to effectively inhibit deep oxidation and improve the selectivity of methacrolein. Generally speaking, the role of additives in the selective oxidation reaction of isobutylene mainly includes the following aspects: reducing the activation energy and enhancing the reaction activity of lattice oxygen in a low temperature environment; improving the activity of the catalyst and enhancing the electron mobility; improving the selectivity of methacrolein; improving the mobility of bulk lattice oxygen; improving the stability of the catalyst, forming a specific crystal phase or synergistic effect, etc.
[0006] However, there are many factors that affect the performance of catalysts. In addition to the elemental composition itself, its microstructure also has a great influence, especially nanoscale catalysts usually show better catalytic performance. Existing molybdenum-bismuth catalysts are all prepared by co-precipitation. During the precipitation process, the particle agglomeration phenomenon is more serious, which affects the uniformity of component distribution and further affects its activity after activation. Therefore, improving the preparation method to make the catalyst powder uniform and fine particles is an important direction that needs to be studied while regulating the elemental composition of the catalyst. Summary of the invention
[0007] In order to solve the problems existing in the above prior art, the present invention provides a high-activity and high-selectivity catalyst for oxidizing isobutylene or tert-butyl alcohol to synthesize methacrolein, and a preparation method and application thereof. The method is to add salts or oxides containing Mo, Bi, Fe, Co, Ni, V, Mg, Sb, Cs, and K to form a dispersed system during the preparation of the catalyst, add a complexing agent and a dispersant to the dispersed system step by step or directly, and promote particle crystallization by slowly hydrolyzing urea in the subsequent crystallization process, so as to control the catalyst morphology, particle size, and uniformity, thereby improving the activity and selectivity of the catalyst.
[0008] One of the objectives of the present invention is to provide a catalyst for the preparation of methacrolein from isobutene or tert-butanol, and the active component of the catalyst has the following general formula:
[0009] Mo a Bi b Fe c Co d Ni e V f Mg g Sb h Cs i K j O x ,
[0010] where a to g are the atomic molar ratios of each element, a = 12, 0 < b < 3.5, 0 < c < 3, 0 < d < 8, 0 ≤ e < 3, 0 ≤ f < 2, 0 < g < 2, 0 < h < 1, 0 < i < 1.5, 0 < j < 2. x is the number of oxygen atoms required to form the composite oxide.
[0011] Another objective of the present invention is to provide a preparation method of a catalyst for the preparation of methacrolein from isobutene or tert-butanol, including the following steps:
[0012] S1. Dissolve the molybdenum-containing compound in water or an acid solution to obtain solution A;
[0013] S2. Dissolve the bismuth-containing compound, iron-containing compound, cobalt-containing compound, magnesium-containing compound, cesium-containing compound, and optionally the nickel-containing compound and vanadium-containing compound in an acid solution, add a complexing agent and a dispersant respectively, and mix and stir to obtain a mixed solution B;
[0014] S3. Disperse the antimony-containing compound and potassium bitartrate in water and heat to obtain solution C;
[0015] S4. Add solution A and solution C to the mixed solution B simultaneously for reaction, and then add a urea solution to obtain a dispersion system D;
[0016] S5. Let the dispersion system D stand and dry to obtain a solid precipitate;
[0017] S6. Activate the solid precipitate to obtain the catalyst matrix powder, and then mix it with a forming aid and form it to obtain the catalyst.
[0018] In the above technical solution, the molybdenum-containing compound, bismuth-containing compound, iron-containing compound, cobalt-containing compound, nickel-containing compound, vanadium-containing compound, magnesium-containing compound, cesium-containing compound, and antimony-containing compound are metal ion precursor compounds, preferably at least one of the oxides, ammonium salts, nitrates, carbonates, bicarbonates, sulfates, halides, oxalates, phosphates, hydrogen phosphates, and complexes thereof of the metals contained therein. The complex may be, for example, an acetylacetone complex.
[0019] In the above technical solution, the complexing agent can be selected from one or more complexing agents such as tartaric acid, citric acid, hydroxybutyric acid, lactic acid, ethylenediaminetetraacetic acid, etc.
[0020] In the above technical solution, the dispersant is an organic alcohol, preferably one or more of methanol, ethanol, ethylene glycol, propylene glycol, glycerol, isopropanol, n-butanol, and isobutanol.
[0021] In the above technical solution, the acid solution may be a dilute nitric acid solution or the like.
[0022] In the above technical scheme, the ratio of the molar amount of the complexing agent to the total molar amount of the metal ions is (0.1-2):1, preferably (0.1-1):1, for example, it can be 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.5:1, 2:1, etc.
[0023] In the above technical scheme, the ratio of the molar amount of the dispersant to the total molar amount of the metal ions is (0.1-2):1, preferably (0.1-1.5):1, for example, it can be 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1.5:1, 2:1, etc.
[0024] In the above technical solution, in step S3, heating to near boiling temperature is performed for a period of time, the near boiling temperature is to control the system temperature to be lower than the boiling temperature <5°C, and the near boiling heating time is 2 to 12 hours, preferably 4 to 8 hours.
[0025] In the above technical solution, in step S3, the antimony-containing compound is a salt or oxide containing Sb, preferably antimony trioxide.
[0026] In the above technical scheme, in step S3, to ensure complete dissolution of the antimony-containing compound, the molar ratio of potassium hydrogen tartrate to antimony in the antimony compound is (1-2):1, preferably (1-1.5):1, for example, it can be 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, etc.
[0027] In the above technical scheme, in step S4, the ratio of the molar amount of urea to the total molar amount of metal ions is (0.01-0.8):1, preferably (0.1-0.7):1, for example, it can be 0.01:1, 0.05:1, 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, etc.
[0028] In the above technical solution, in step S4, the reaction temperature is preferably 40 to 90° C., preferably 50 to 80° C., and the reaction time is 0.5 to 10 h, preferably 1 to 6 h.
[0029] In the above technical solution, in step S5, the standing temperature is 0 to 150° C., preferably 20 to 150° C.; the standing time is 6 to 24 hours, preferably 6 to 12 hours; and the pH of the solution after standing is 0 to 8, preferably 1 to 7.
[0030] In the above technical solution, in step S5, the drying temperature is 100-200° C., preferably 100-150° C.; the drying time is 12-36 hours, preferably 18-24 hours.
[0031] In the above technical solution, in step S6, the activation process is to calcine the obtained solid precipitate at 200-300°C for 1-6h, preferably 2-4h, and then continue to heat up to 450-550°C with or without changing the atmosphere, and keep at this temperature for 2-10h, preferably 2-6h. Then, the obtained sample is mixed with a molding aid and further molded to obtain the catalyst for oxidizing isobutylene or tert-butyl alcohol to prepare methacrolein.
[0032] In the above technical solution, in step S6, there is no particular limitation on the molding aid, and commonly used molding aids such as graphite can be selected. The amount of the molding aid can be selected from the usual amount in the art.
[0033] According to a preferred embodiment of the present invention, the technical solution of the method for preparing the catalyst for preparing methacrolein from isobutylene or tert-butyl alcohol comprises the following steps:
[0034] S1. According to the catalyst formula ratio, dissolve an appropriate amount of molybdenum-containing compound in an appropriate amount of deionized water or dilute nitric acid solution to obtain a metal salt solution A;
[0035] S2. According to the catalyst formulation ratio, an appropriate amount of metal ion precursor compounds such as Bi, Fe, Co, Ni, V, Mg, Cs, etc. are dissolved in a dilute nitric acid solution, and a certain amount of a complexing agent and a dispersant are added thereto respectively, mixed and stirred to obtain a mixed solution B;
[0036] S3. According to the catalyst formula ratio, an appropriate amount of Sb precursor compound and a certain amount of potassium hydrogen tartrate are dispersed in water in a certain ratio, heated to near boiling and reacted for a period of time to obtain solution C;
[0037] S4, adding solution A and solution C to the mixed solution B at the same time, reacting at a certain temperature for a certain time, and then adding a certain amount of urea aqueous solution thereto to obtain a dispersed system D;
[0038] S5, transferring the dispersed system D to a hydrothermal reactor, standing the system for a certain period of time at a certain temperature, utilizing the slow decomposition of urea under the preferred temperature conditions to precipitate the metal ions from the metal chelate, and generating metal oxides with good crystallinity in the hydrothermal environment, evaporating the water in the system, and drying the obtained solid precipitate at a certain temperature;
[0039] S6. Prepare a solid shaped catalyst, precipitate the obtained solid, activate it through a certain activation process to obtain a catalyst matrix powder sample, mix it with a certain amount of molding aid such as graphite, and further shape it to obtain the catalyst.
[0040] The third object of the present invention is to provide a catalyst obtained by the above-mentioned preparation method.
[0041] A fourth object of the present invention is to provide a method for preparing methacrolein from isobutylene or tert-butyl alcohol, wherein the catalyst or the catalyst obtained by the preparation method is used.
[0042] The method comprises subjecting isobutylene or tert-butyl alcohol to an oxidation reaction in the presence of the molybdenum bismuth oxygen catalyst.
[0043] According to a preferred embodiment of the present invention, the catalyst provided by the present invention is used in a fixed bed reactor to catalyze the reaction of gas phase selective catalytic oxidation of isobutylene / tert-butyl alcohol to synthesize methacrolein, and the reaction conditions are: reaction temperature of 300-400° C., isobutylene or tert-butyl alcohol 3-10% by volume, and space velocity of 500-3000 h -1 , the pressure is 0.01~0.2MPa.
[0044] The preparation method of the catalyst for preparing methacrolein by oxidation of isobutylene or tert-butyl alcohol of the present invention uses a complexing agent as a synthetic reaction template, improves the uniformity of the system components by a dispersant, and further uniformly precipitates the metal ions in the system by controlling the decomposition of urea to generate a mixture of molybdenum and bismuth oxides, and continues to age under hydrothermal conditions to improve the crystallinity of the grains. The obtained solid precipitate breaks the CO-metal bond during activation, and the unreacted urea decomposes, while NH3 and CO2 escape, thereby generating a large number of pores on the particle surface, which is conducive to the formation of nanoporous oxide particles. The method is simple to operate, has low equipment requirements, and does not require a strict physical environment during the preparation process; the reactants can be uniformly mixed in the liquid phase to obtain a uniform multi-component dispersion system, which is convenient for controlling the chemical composition of the powder; effectively reduces the agglomeration of the powder, and the precipitation of ions in the solution can be relatively uniformly controlled by the slow decomposition of urea; the powder particle size is small, and pores can be formed on the particle surface by decomposing the organic components in the subsequent activation process, thereby increasing the specific surface area of the particles.
[0045] The beneficial effects of the present invention are as follows: the catalyst provided by the present invention is used in a fixed bed reactor to catalyze the reaction of synthesizing methacrolein by gas phase selective catalytic oxidation of isobutylene / tert-butyl alcohol, at a reaction temperature of 300-400° C., isobutylene / tert-butyl alcohol 3-10% by volume, and a space velocity of 500-3000 h -1 Under the condition of pressure of 0.01-0.2MPa, the conversion rate of isobutylene / tert-butyl alcohol is 95.0-99.0%, and the selectivity of methacrolein reaches 87.1-89.8%; under the same conditions, the molybdenum bismuth oxygen catalyst without adding complexing agent and dispersant and promoted by urea hydrothermal decomposition has a catalytic performance of isobutylene / tert-butyl alcohol conversion rate of 91.1-96.8%, and methacrolein selectivity reaches 83.9-89.0%. By using the catalyst of the present invention, the conversion rate of isobutylene / tert-butyl alcohol can be increased by up to 3.8%, and the total selectivity of methacrolein and methacrylic acid can be increased by up to 4.9%. DETAILED DESCRIPTION
[0046] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0047] The raw materials used in the examples and comparative examples, unless otherwise specified, are disclosed in the prior art, for example, they can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0048] The catalyst performance evaluation experiment was completed on a fixed bed reactor, where the reactor tube is 70cm long, the inner diameter is 25mm, and a temperature measuring couple tube with an outer diameter of 6mm is built in. The catalyst loading is 120mL and the loading height is 30cm. Air and isobutylene are measured by mass flow meters, and tert-butyl alcohol is measured by precision metering pumps before entering the reaction tube. A branch is installed at the inlet to analyze the composition of the raw gas by gas chromatography. The reaction gas is selectively oxidized under the action of the activated catalyst to generate selective target products. A branch is installed at the tail gas outlet to analyze the composition of the tail gas. Chromatographic analysis is performed using an Agilent 7890b gas chromatograph from the United States. The data used in the following discussion are all data with a carbon balance between 98% and 102%.
[0049] According to the present invention, the contact conditions can be selected in a wide range, but in order to further improve the selectivity of methacrolein and methacrylic acid, preferably, the contact conditions include: temperature of 300-400°C, pressure of 0.01-0.2MPa, reaction time of 1-48h, total volume space velocity of raw materials of 500-3000h -1 , preferably 800~2000h -1 ; The molar ratio of isobutylene: oxygen: water in the raw material is 1:1-5:2-6. Alternatively, the contact conditions include: temperature of 300-400°C, pressure of 0.01-0.2 MPa, reaction time of 1-48 hours, space velocity of 500-3000 h -1 , preferably 800~2000h -1 ; The molar ratio of tert-butanol: oxygen in the raw material is 1:1~5:1~5.
[0050] The calculation of the raw material conversion rate and the selectivity of the generated products during the reaction is as follows:
[0051]
[0052]
[0053]
[0054] Example 1
[0055] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A; 0.024 mol of bismuth nitrate, 0.047 mol of iron nitrate, 0.186 mol of cobalt nitrate, 0.005 mol of nickel nitrate, 0.012 mol of magnesium nitrate, 0.009 mol of cesium nitrate, and 0.016 mol of ammonium metavanadate were dissolved in 100 mL of 60°C deionized water. 15% nitric acid solution, after the solution is clear and transparent, add 0.070mol tartaric acid, after the tartaric acid is completely dissolved, add 6g ethylene glycol to obtain solution B; 0.012mol potassium hydrogen tartrate and 0.006mol antimony trioxide are dispersed in 20mL deionized water, heated to 98℃, reacted for 4 hours, and obtained solution C; solution A and solution C are added to solution B at the same time, and stirred continuously in a 60℃ water bath for 4 hours; 50mL urea solution containing 0.2mol urea is added to the above dispersion system; the dispersion system is transferred to a hydrothermal autoclave, and after standing at 120℃ for 6h, the pH value of the system is 1.42, and dried at 140℃ for 24h; the obtained solid is heated to 300℃ in a tube furnace at 2℃ / min and roasted for 3h, and then continued to heat to 450℃ and roasted for 5h. The composition of the catalyst is shown in Table 1. After adding graphite in a mass ratio of 4 / 96 to the catalyst matrix powder and mixing evenly, the mixture was punched into a hollow cylinder with an outer diameter of 5 mm, an inner diameter of 2 mm, and a height of 4 mm on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0056] Example 2
[0057] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A; 0.035 mol of bismuth nitrate, 0.024 mol of iron nitrate, 0.160 mol of cobalt nitrate, 0.023 mol of magnesium nitrate, 0.014 mol of cesium nitrate, and 0.033 mol of ammonium metavanadate were dissolved in 100 mL of 60°C deionized water; 15% nitric acid solution, after the solution is clear and transparent, add 0.168mol citric acid, after the citric acid is completely dissolved, add 30g ethylene glycol to obtain solution B; 0.016mol potassium hydrogen tartrate and 0.007mol antimony trioxide are dispersed in 25mL deionized water, heated to 98℃, reacted for 5 hours, and obtained solution C; solution A and solution C are added to solution B at the same time, and stirred continuously in a 60℃ water bath for 4 hours; 50mL urea solution containing 0.4mol urea is added to the above dispersion system; the dispersion system is transferred to a hydrothermal autoclave, and after standing at 130℃ for 8h, the pH value of the system is 5.07, and dried at 100℃ for 36h; the obtained solid is heated to 300℃ in a tube furnace at 2℃ / min and roasted for 4h, and then continued to heat to 450℃ and roasted for 5h. The composition of the catalyst is shown in Table 1. After adding graphite in a mass ratio of 4 / 96 to the catalyst matrix powder and mixing evenly, the mixture was punched into a hollow cylinder with an outer diameter of 5 mm, an inner diameter of 2 mm, and a height of 4 mm on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0058] Example 3
[0059] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A; 0.047 mol of bismuth nitrate, 0.069 mol of ferric nitrate, 0.066 mol of cobalt nitrate, 0.036 mol of magnesium nitrate, 0.021 mol of cesium nitrate, and 0.012 mol of ammonium metavanadate were dissolved in 100 mL of 60°C deionized water. 15% nitric acid solution, after the solution is clear and transparent, add 0.67mol tartaric acid, after the tartaric acid is completely dissolved, add 40g ethylene glycol to obtain solution B; 0.014mol potassium hydrogen tartrate and 0.006mol antimony trioxide are dispersed in 25mL deionized water, heated to 98℃, reacted for 5 hours, and obtained solution C; solution A and solution C are added to solution B at the same time, and stirred continuously in a 60℃ water bath for 4 hours; 50mL urea solution containing 0.43mol urea is added to the above dispersion system; the dispersion system is transferred to a hydrothermal autoclave, and after standing at 135℃ for 12h, the pH value of the system is 6.04, and dried at 180℃ for 18h; the obtained solid is heated to 300℃ in a tube furnace at 2℃ / min and roasted for 3h, and then continued to heat to 500℃ and roasted for 5h. The composition of the catalyst is shown in Table 1. After adding graphite in a mass ratio of 5 / 95 to the catalyst matrix powder and mixing evenly, the mixture was punched into a hollow cylinder with an outer diameter of 5 mm, an inner diameter of 2 mm, and a height of 4 mm on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0060] Example 4
[0061] Dissolve 0.040 mol of ammonium heptamolybdate in 100 mL of 60°C deionized water to obtain solution A; dissolve 0.071 mol of bismuth nitrate, 0.035 mol of iron nitrate, 0.111 mol of cobalt nitrate, 0.033 mol of nickel nitrate, 0.038 mol of magnesium nitrate, and 0.033 mol of cesium nitrate in 100 mL of 15% nitric acid solution, after the solution is clear and transparent, add 0.53 mol citric acid, after the citric acid is completely dissolved, add 50g ethylene glycol to obtain solution B; 0.017 mol potassium hydrogen tartrate and 0.007 mol antimony trioxide are dispersed in 30mL deionized water, heated to 98°C, reacted for 6 hours, and obtained solution C; solution A and solution C are added to solution B at the same time, and stirred continuously in a 60°C water bath for 4 hours; 50mL urea solution containing 0.5 mol urea is added to the above dispersion system; the dispersion system is transferred to a hydrothermal autoclave, and after standing at 145°C for 24 hours, the pH value of the system is 7.18, and it is dried at 140°C for 24 hours; the obtained solid is heated to 300°C in a tube furnace at 2°C / min and roasted for 2 hours, and then continued to heat to 550°C and roasted for 5 hours. The composition of the catalyst is shown in Table 1. Graphite was added to the catalyst matrix powder in a mass ratio of 4 / 96 and mixed evenly, and then pressed into a 6 mm diameter clover-shaped cylinder on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0062] Example 5
[0063] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A. 0.054 mol of bismuth nitrate, 0.068 mol of ferric nitrate, 0.083 mol of cobalt nitrate, 0.012 mol of nickel nitrate, 0.021 mol of magnesium nitrate and 0.024 mol of cesium nitrate were dissolved in 100 mL of 15% nitric acid solution at 60°C. After the solution became clear, 0.137 mol of EDTA, after EDTA is completely dissolved, add 50g of ethylene glycol to obtain solution B; disperse 0.018mol potassium hydrogen tartrate and 0.005mol antimony trioxide in 30mL deionized water, heat to 98℃, react for 6 hours, and obtain solution C; add solution A and solution C to solution B at the same time, and continue stirring in a 60℃ water bath for 4 hours; add 50mL of urea solution containing 0.3mol urea to the above dispersion system; transfer the dispersion system to a hydrothermal autoclave, stand for reaction at 140℃ for 12h, the pH value of the system is 4.41, and dry at 150℃ for 24h; heat the obtained solid to 300℃ in a tube furnace at 2℃ / min and roast for 2h, and then continue to heat to 480℃ and roast for 5h. The composition of the catalyst is shown in Table 1. Graphite was added to the catalyst matrix powder in a mass ratio of 5 / 95 and mixed evenly, and then pressed into a 6 mm diameter clover-shaped cylinder on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0064] Example 6
[0065] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A; 0.080 mol of bismuth nitrate, 0.049 mol of ferric nitrate, 0.040 mol of cobalt nitrate, 0.061 mol of nickel nitrate, 0.045 mol of magnesium nitrate, 0.013 mol of ammonium metavanadate, and 0.009 mol of cesium nitrate were dissolved in 100 mL of 15% nitric acid solution at 60°C. After the solution became clear, 0.27 mol of EDTA, after EDTA is completely dissolved, add 50g of ethylene glycol to obtain solution B; disperse 0.020mol potassium hydrogen tartrate and 0.007mol antimony trioxide in 30mL deionized water, heat to 98℃, react for 6 hours, and obtain solution C; add solution A and solution C to solution B at the same time, and continue stirring in a 60℃ water bath for 4 hours; add 50mL of urea solution containing 0.43mol urea to the above dispersion system; transfer the dispersion system to a hydrothermal autoclave, stand for reaction at 145℃ for 12h, the pH value of the system is 6.12, dry at 140℃ for 26h; heat the obtained solid to 300℃ in a tube furnace at 2℃ / min and roast for 3h, then continue to heat to 530℃ and roast for 5h. The composition of the catalyst is shown in Table 1. Graphite was added to the catalyst matrix powder in a mass ratio of 4 / 96 and mixed evenly, and then pressed into a cylinder with an outer diameter of 5 mm and a height of 4 mm on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0066] Example 7
[0067] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A; 0.024 mol of bismuth nitrate, 0.047 mol of iron nitrate, 0.117 mol of cobalt nitrate, 0.012 mol of magnesium nitrate, 0.028 mol of cesium nitrate, and 0.016 mol of ammonium metavanadate were dissolved in 100 mL of 60°C deionized water. 15% nitric acid solution, after the solution is clear and transparent, add 0.07mol tartaric acid, after the tartaric acid is completely dissolved, add 6g ethylene glycol to obtain solution B; 0.041mol potassium hydrogen tartrate and 0.011mol antimony trioxide are dispersed in 20mL deionized water, heated to 98℃, reacted for 4 hours, and obtained solution C; solution A and solution C are added to solution B at the same time, and 50mL urea solution containing 0.2mol urea is added thereto, and then stirred continuously in a water bath at 80℃ for 4 hours, and the system is transferred to a hydrothermal kettle, and after standing at 150℃ for 6h, the pH value of the system is 2.98, and dried at 140℃ for 26h; the obtained solid is heated to 300℃ in a tube furnace at 2℃ / min and roasted for 3h, and then continued to heat to 500℃ and roasted for 5h. The composition of the catalyst is shown in Table 1. Graphite was added to the catalyst matrix powder in a mass ratio of 4 / 96 and mixed evenly, and then pressed into a cylinder with an outer diameter of 5 mm and a height of 4 mm on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0068] Comparative Example 1
[0069] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A; 0.024 mol of bismuth nitrate, 0.047 mol of iron nitrate, 0.186 mol of cobalt nitrate, 0.005 mol of nickel nitrate, 0.012 mol of magnesium nitrate, 0.009 mol of cesium nitrate, and 0.016 mol of ammonium metavanadate were dissolved in 100 mL of 60°C deionized water. 15% nitric acid solution to obtain solution B; 0.012mol potassium hydrogen tartrate and 0.006mol antimony trioxide were dispersed in 20mL deionized water, heated to 98°C, reacted for 4 hours, and solution C was obtained; solution A and solution C were added to solution B at the same time, and after continuous stirring in a 60°C water bath for 4 hours, the pH value of the system was less than 1, which was strongly acidic, and dried at 140°C for 24h; the obtained solid was heated to 300°C in a tube furnace at 2°C / min for 3h, and then continued to heat to 450°C for 5h. The composition of the catalyst is shown in Table 1. After adding graphite with a mass ratio of 4 / 96 to the catalyst matrix powder and mixing evenly, it was punched into a hollow cylinder with an outer diameter of 5mm, an inner diameter of 2mm, and a height of 4mm on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0070] Comparative Example 2
[0071] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A; 0.035 mol of bismuth nitrate, 0.024 mol of iron nitrate, 0.160 mol of cobalt nitrate, 0.023 mol of magnesium nitrate, 0.014 mol of cesium nitrate, and 0.033 mol of ammonium metavanadate were dissolved in 100 mL of 60°C deionized water; In a 15% nitric acid solution, after the solution becomes clear and transparent, 0.168 mol of citric acid is added. After the citric acid is completely dissolved, 30 g of ethylene glycol is added thereto to obtain solution B; 0.016 mol of potassium hydrogen tartrate and 0.007 mol of antimony trioxide are dispersed in 20 mL of deionized water, heated to 98 ° C, and reacted for 4 hours to obtain solution C; solution A and solution C are added to solution B at the same time, and after continuous stirring in a 60 ° C water bath for 4 hours, the pH value of the system is less than 1, which is strongly acidic, and dried at 140 ° C for 24 hours; the obtained solid is heated to 300 ° C in a tube furnace at 2 ° C / min and roasted for 4 hours, and then continued to heat to 450 ° C and roasted for 5 hours. The composition of the catalyst is shown in Table 1. After adding graphite with a mass ratio of 4 / 96 to the catalyst matrix powder and mixing evenly, it is punched into a hollow cylinder with an outer diameter of 5 mm, an inner diameter of 2 mm, and a height of 4 mm on a tablet press. The obtained shaped catalyst was loaded into a fixed bed reactor for evaluation. The catalytic performance is shown in Table 2.
[0072] Comparative Example 3
[0073] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A; 0.047 mol of bismuth nitrate, 0.069 mol of ferric nitrate, 0.066 mol of cobalt nitrate, 0.036 mol of magnesium nitrate, 0.021 mol of cesium nitrate, and 0.012 mol of ammonium metavanadate were dissolved in 100 mL of 60°C deionized water. 15% nitric acid solution to obtain solution B; 0.014 mol potassium hydrogen tartrate and 0.006 mol antimony trioxide were dispersed in 25 mL deionized water, heated to 98 ° C, and reacted for 5 hours to obtain solution C; solution A and solution C were added to solution B at the same time, and stirred continuously in a 60 ° C water bath for 4 hours; 50 mL of urea solution containing 0.43 mol urea was added to the above dispersion system; the dispersion system was transferred to a hydrothermal autoclave, and after standing and reacting at 135 ° C for 12 hours, the pH value of the system was 6.09, and dried at 180 ° C for 18 hours; the obtained solid was heated to 300 ° C in a tube furnace at 2 ° C / min and roasted for 3 hours, and then continued to heat to 500 ° C and roasted for 5 hours. The composition of the catalyst is shown in Table 1. After adding graphite in a mass ratio of 5 / 95 to the catalyst matrix powder and mixing evenly, the mixture was punched into a hollow cylinder with an outer diameter of 5 mm, an inner diameter of 2 mm, and a height of 4 mm on a tablet press. The resulting shaped catalyst was loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0074] Comparative Example 4
[0075] Dissolve 0.040 mol of ammonium heptamolybdate in 100 mL of 60°C deionized water to obtain solution A; dissolve 0.071 mol of bismuth nitrate, 0.035 mol of iron nitrate, 0.111 mol of cobalt nitrate, 0.033 mol of nickel nitrate, 0.038 mol of magnesium nitrate, and 0.033 mol of cesium nitrate in 100 mL of 15% nitric acid solution, after the solution is clear and transparent, add 0.53 mol citric acid to obtain solution B; add solution A to solution B, add 0.007 mol antimony trioxide to it, and continue to stir in a 60°C water bath for 4 hours; add 50 mL of urea solution containing 0.5 mol urea to the above dispersion system; transfer the dispersion system to a hydrothermal kettle, stand at 145°C for 24 hours, the pH value of the system is 7.07, and dry at 140°C for 24 hours; heat the obtained solid to 300°C in a tube furnace at 2°C / min and roast for 2 hours, and then continue to heat to 500°C and roast for 5 hours. The composition of the catalyst is shown in Table 1. After adding graphite with a mass ratio of 4 / 96 to the catalyst matrix powder and mixing evenly, it is punched into a 6 mm outer diameter and a clover-shaped cross-section on a tablet press. The resulting molded catalyst is loaded into a fixed bed reactor for evaluation, and the catalytic performance is shown in Table 2.
[0076] Comparative Example 5
[0077] 0.040 mol of ammonium heptamolybdate was dissolved in 100 mL of 60°C deionized water to obtain solution A. 0.054 mol of bismuth nitrate, 0.068 mol of ferric nitrate, 0.083 mol of cobalt nitrate, 0.012 mol of nickel nitrate, 0.021 mol of magnesium nitrate and 0.024 mol of cesium nitrate were dissolved in 100 mL of 15% nitric acid solution at 60°C. After the solution became clear, 0.137 mol of EDTA, after EDTA is completely dissolved, 50g of ethylene glycol is added thereto to obtain solution B; 0.018mol potassium hydrogen tartrate and 0.005mol antimony trioxide are dispersed in 30mL and deionized water, heated to 98°C, reacted for 6 hours, and solution C is obtained; solution A and solution C are added to solution B at the same time, and 50mL of urea solution containing 0.3mol urea is added thereto, and then stirred in a 60°C water bath for 4 hours, the pH value of the system is 3.23, and dried at 150°C for 24h; the obtained solid is heated to 300°C in a tube furnace at 2°C / min and roasted for 2h, and then continued to heat to 480°C and roasted for 5h. The composition of the catalyst is shown in Table 1. After adding graphite with a mass ratio of 5 / 95 to the catalyst matrix powder and mixing evenly, it is punched into a 6mm outer diameter and a clover-shaped cross-section on a tablet press. The obtained shaped catalyst was loaded into a fixed bed reactor for evaluation. The catalytic performance is shown in Table 2.
[0078] Table 1 Catalyst compositions
[0079]
[0080] Example 8
[0081] The catalysts prepared in Examples 1-7 and Comparative Examples 1-5 were loaded into a fixed bed reactor as selective oxidation catalysts for oxidation of isobutylene / tert-butyl alcohol to methacrolein / acid, and the catalyst performance was tested at a reaction temperature of 360°C.
[0082] The catalytic results are shown in Table 2 after online gas chromatography analysis. The evaluation method adopts but is not limited to the above conditions.
[0083] Table 2 Catalytic performance of catalysts for selective oxidation of isobutylene / tert-butyl alcohol to methacrolein / acid
[0084]
[0085] aThe raw materials are isobutylene: oxygen: nitrogen: water
[0086] b The raw materials are tert-butyl alcohol: oxygen: nitrogen: water
[0087] In the catalyst preparation process of the present invention, a complexing agent and a dispersant are added to a salt or oxide dispersion system containing Mo, Bi, Fe, Co, Mg, V, Sb, Cs, K, and Ni, and urea is slowly hydrolyzed in the subsequent crystallization process to promote the crystallization of particles, thereby achieving the purpose of controlling the catalyst morphology, particle size, and uniformity, thereby improving the activity and selectivity of the catalyst.
[0088] Any numerical value mentioned in the present invention, if there is only an interval of two units between any minimum value and any maximum value, includes all values from the minimum value to the maximum value each time increasing by one unit. For example, if the amount of a component, or the value of a process variable such as temperature, pressure, time, etc. is declared to be 50-90, in this specification it means that 51-89, 52-88... and 69-71 and 70-71 are specifically listed. For non-integer values, 0.1, 0.01, 0.001 or 0.0001 can be appropriately considered as a unit. These are just some specially specified examples. In this application, in a similar manner, all possible combinations of numerical values between the listed minimum and maximum values are considered to have been disclosed.
[0089] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A catalyst for preparing methacrolein from isobutylene or tert-butyl alcohol, wherein the active component of the catalyst has the following general formula: Mo a Bi b Feb c Co d Ni e V f Mg g Sb h Cs i K j O x , in, a=12,0 <b<3.5,0<c<3,0<d<8,0≤e<3,0≤f<2,0<g<2,0<h<1,0<i<1.5,0<j<2; The preparation method of the catalyst comprises the following steps: S1, dissolving a molybdenum-containing compound in water or an acid solution to obtain a solution A; S2, dissolving a bismuth-containing compound, an iron-containing compound, a cobalt-containing compound, a magnesium-containing compound, a cesium-containing compound, and an optional nickel-containing compound and a vanadium-containing compound in an acid solution, and respectively adding a complexing agent and a dispersant to obtain a mixed solution B; S3, dispersing an antimony-containing compound and potassium hydrogen tartrate in water, and heating to obtain a solution C; S4, adding solution A and solution C to the mixed solution B at the same time, reacting, and then adding a urea solution to obtain a dispersed system D; S5, allowing the dispersed system D to stand and dry to obtain a solid precipitate; S6, activating the solid precipitate to obtain a catalyst matrix powder, and then mixing it with a molding aid to mold it to obtain the catalyst.
2. A method for preparing the catalyst according to claim 1, comprising the following steps: S1, dissolving the molybdenum-containing compound in water or an acid solution to obtain a solution A; S2, dissolving a bismuth-containing compound, an iron-containing compound, a cobalt-containing compound, a magnesium-containing compound, a cesium-containing compound, and an optional nickel-containing compound and a vanadium-containing compound in an acid solution, and adding a complexing agent and a dispersant respectively to obtain a mixed solution B; S3, dispersing the antimony-containing compound and potassium hydrogen tartrate in water, and heating to obtain solution C; S4, adding solution A and solution C to the mixed solution B simultaneously to react, and then adding urea solution to obtain a dispersed system D; S5, allowing the dispersed system D to stand and dry to obtain a solid precipitate; S6. Activate the solid precipitate to obtain catalyst matrix powder, then mix it with a molding aid and mold it to obtain the catalyst.
3. The method for preparing the catalyst according to claim 2, characterized in that: The molybdenum-containing compound, bismuth-containing compound, iron-containing compound, cobalt-containing compound, nickel-containing compound, vanadium-containing compound, magnesium-containing compound, cesium-containing compound, and antimony-containing compound are at least one of the oxides, ammonium salts, nitrates, carbonates, bicarbonates, sulfates, halides, oxalates, phosphates, hydrogen phosphates, and complexes thereof of the metals contained therein; and / or, The complexing agent is at least one of tartaric acid, citric acid, hydroxybutyric acid, lactic acid, and ethylenediaminetetraacetic acid; and / or, The dispersant is an organic alcohol.
4. The method for preparing the catalyst according to claim 3, characterized in that: The dispersant is at least one of methanol, ethanol, ethylene glycol, propylene glycol, glycerol, isopropanol, n-butanol, and isobutanol.
5. The method for preparing the catalyst according to claim 2, characterized in that: The ratio of the molar amount of the complexing agent to the total molar amount of the metal ions is (0.1-2):1; and / or, The ratio of the molar amount of the dispersant to the total molar amount of the metal ions is (0.1-2):
1.
6. The method for preparing the catalyst according to claim 5, characterized in that: The ratio of the molar amount of the complexing agent to the total molar amount of the metal ions is (0.1-1):1; and / or, The ratio of the molar amount of the dispersant to the total molar amount of the metal ions is (0.1-1.5):
1.
7. The method for preparing the catalyst according to claim 2, characterized in that In step S3: The molar ratio of potassium hydrogen tartrate to the antimony in the antimony-containing compound is (1-2):1; The temperature of the heating control system is at least 5°C below the boiling temperature; The heating time is 2 to 12 hours.
8. The method for preparing the catalyst according to claim 7, characterized in that: The molar ratio of potassium hydrogen tartrate to the antimony in the antimony-containing compound (1 to 1.5): 1; The heating time is 4 to 8 hours.
9. The method for preparing the catalyst according to claim 2, characterized in that In step S4: The ratio of the molar amount of urea to the total molar amount of metal ions is (0.01-0.8):1; The reaction temperature is 40-90°C; The reaction time is 0.5 to 10 hours.
10. The method for preparing the catalyst according to claim 9, characterized in that: The ratio of the molar amount of urea to the total molar amount of metal ions is (0.1-0.7):1; The reaction temperature is 50-80°C; The reaction time is 1 to 6 hours.
11. The method for preparing the catalyst according to claim 2, characterized in that In step S5: The standing temperature is 0~150℃; The standing time is 6 to 24 hours; The pH of the solution after standing is 0-8; Drying temperature is 100-200°C; The drying time is 12 to 36 hours.
12. The method for preparing the catalyst according to claim 11, characterized in that: The standing temperature is 20~150℃; The standing time is 6 to 12 hours; The pH of the solution after standing is 1 to 7; Drying temperature is 100-150°C; The drying time is 18 to 24 hours.
13. The method for preparing the catalyst according to claim 2, characterized in that In step S6: The activation comprises calcining the solid precipitate at 200-300° C. for 1-6 hours, and then continuing to heat the solid precipitate to 450-550° C. with or without changing the atmosphere, and maintaining the solid precipitate at this temperature for 2-10 hours.
14. The method for preparing the catalyst according to claim 13, characterized in that: The activation comprises calcining the solid precipitate at 200-300° C. for 2-4 hours, and then continuing to heat the solid precipitate to 450-550° C. with or without changing the atmosphere, and maintaining the solid precipitate at this temperature for 2-6 hours.
15. The catalyst obtained according to the preparation method according to any one of claims 2 to 14.