A high-strength wear-resistant super-hydrophobic powder and preparation method thereof

The preparation of superhydrophobic powder by the melting method solves the problems of pollution, expensive equipment and low strength in the preparation of superhydrophobic materials in the existing technology, and achieves high-strength and wear-resistant superhydrophobic powder, which is suitable for building materials and improves the performance of cement mortar. .

CN116553854BActive Publication Date: 2024-10-29YELLOW RIVER ENG CONSULTING CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310584489.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-10-29
Estimated Expiration
2043-05-23

AI Technical Summary

Technical Problem

Existing superhydrophobic material preparation methods have problems such as pollution, expensive equipment, complex processes, low strength, and lack of wear resistance, making it difficult to achieve high-strength and wear-resistant industrial production.

Method used

The melting method is used to stir, heat, cool and vacuum-dry the mineral admixture micron powder, nano-silica and long-chain fatty acids in a specific ratio to form a high-strength and wear-resistant super-hydrophobic powder.

Benefits of technology

A low-cost, environmentally friendly, simple and easy preparation of super-hydrophobic powder is achieved, which improves the pressure resistance and anti-wear capabilities of cement mortar and has good hydrophobic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116553854B_ABST
    Figure CN116553854B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a high-strength wear-resistant super-hydrophobic powder, which is prepared by a melting method from 40 to 70 parts of raw material mineral admixture powder, 10 to 50 parts of nano silicon dioxide, and 5 to 30 parts of long-chain fatty acid powder: the mineral admixture and the long-chain fatty acid are accurately weighed according to the above weight parts, put into a stirrer, and stirred evenly at a low speed, and then gradually heated to 80 to 160 degrees Celsius. o C, keep the temperature high-speed stirring for 10~30 min, then add weighed nano silicon dioxide, continue high-speed stirring for 10~20 min and stop heating, cool the powder to room temperature under stirring, then vacuum dry, finally grind to a certain fineness to obtain a high-strength wear-resistant super hydrophobic powder finished product. The invention has the advantages that the modification method is simple, environmentally friendly, low in production cost, easy to operate, without expensive instruments and harsh process conditions, the obtained finished powder is mixed in cement mortar as an additive, the compression resistance and wear resistance of cement mortar can be greatly improved, and it has good hydrophobic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to functional materials for the construction field, and in particular to a method for preparing high-strength wear-resistant super-hydrophobic powder. Background Art

[0002] Learning from nature and inspired by the "lotus effect" in nature, superhydrophobic materials have received more and more attention. Superhydrophobic materials have broad application prospects in daily life and industrial and agricultural production because of their waterproof, anti-fouling, anti-icing, self-cleaning, and corrosion resistance. Generally, there are two methods to prepare superhydrophobic surfaces. One is to construct a microscopic rough structure on the surface of the hydrophobic material; the other is to modify the microscopic rough surface with a low surface energy substance. Currently, the commonly used preparation methods include etching, vapor deposition, electrospinning technology, sol-gel method, etc. Although the mechanism has been clarified, there are still many constraints in the preparation of superhydrophobic materials. For example, fluorine-containing substances that pollute the environment are used in the preparation process; the preparation process is complicated and requires expensive equipment; the preparation process is still in the laboratory stage and cannot be industrialized; superhydrophobic materials have low strength and are not wear-resistant. Therefore, while meeting the requirements of high strength and wear resistance, it is an inevitable trend to use a simpler and more environmentally friendly method to prepare rough micro-nano structures with low surface energy.

[0003] Patent CN111777736A discloses a super-hydrophobic powder material, with tetrahydrofuran as solvent, under heated stirring and inert gas protection conditions, isocyanate and hydroxy silicone oil are fully mixed and chemically reacted, after the system temperature is cooled, the tetrahydrofuran solution of chain extender and catalyst mixed is slowly added, and stirring is continued until the reaction terminates, and the reaction product is poured into the precipitated phase afterwards, and suction filtration is separated, and the separated material is dried and ground, and finally super-hydrophobic powder is obtained. The method reaction conditions are complicated, and unnecessary chemical components are introduced, and a fine separation process is required, otherwise pollution will be caused in use, and it is difficult for large-scale preparation. Patent CN108424020B discloses a super-hydrophobic modification method of a mineral admixture, with the mixed solution of cyclohexane-n-butanol as solvent, the ethanol / water solution of silane coupling agent is added thereto, and silicone oil modifier is added dropwise, and super-hydrophobic modified mineral admixture is obtained after dry grinding. This method is a wet modification, and uses expensive silane coupling agents, etc., and a large amount of organic solvents will be used at the same time, which will have a certain impact on the environment when mass-producing powders. Patent CN104672962A discloses an inorganic super-hydrophobic coating, which uses polymer nanoparticles such as polystyrene / polymethyl acrylate as a template, and the hydrosol after hydrolysis of tetraethoxysilane hydrochloride is the mother liquor, which is injected into the template to form a gel, and then the polymer microspheres are removed by hydrolysis or calcination. The obtained powder is ground and reacted with a silane coupling agent to obtain a super-hydrophobic powder modified with a micro-nano structure and low surface energy groups. This method has complex steps and requires 600 oThe high temperature heating above C to remove the polymer template still presents certain technical difficulties when mass production is required.

[0004] Therefore, in view of the shortcomings of the current existing technology, it is urgent to design a preparation method that is safe, environmentally friendly, simple to operate, low-cost, and does not require expensive instruments and strict process conditions to produce high-strength and wear-resistant superhydrophobic powder suitable for the construction field. Summary of the invention

[0005] The purpose of the present invention is to provide a super-hydrophobic powder preparation technology which is low in price, superior in performance and can be used for building materials, in view of the current problems of high cost and limited use of super-hydrophobic powder preparation. The preparation method is simple and easy to implement, and is easy to realize large-scale production. It is green, energy-saving and environmentally friendly, and has good social and economic benefits.

[0006] To achieve the above purpose, the present invention can adopt the following technical solutions:

[0007] The method for preparing the high-strength wear-resistant super-hydrophobic powder of the present invention is to prepare the powder by melting the raw material mineral admixture powder, nano silicon dioxide and long-chain fatty acid powder according to the following weight ratio:

[0008] Proportion: 40-70 parts of mineral admixture powder, 10-50 parts of nano-silicon dioxide, 5-30 parts of long-chain fatty acid powder;

[0009] Preparation method: accurately weigh the mineral admixture and long-chain fatty acid according to the above weight, put them into a stirrer and stir them evenly at a low speed, then gradually heat them to 80~160 o C (determined by the long-chain fatty acid used), maintain the temperature and stir at high speed for 10 to 30 minutes, then add the weighed nano-silica, continue to stir at high speed for 10 to 20 minutes and then stop heating, cool the powder to room temperature under stirring, then perform vacuum drying, and finally grind to a certain fineness (800-1000 mesh) to obtain a high-strength, wear-resistant and super-hydrophobic powder product.

[0010] The mineral admixture powder used in the present invention is a mixed powder of one or more of mica powder, corundum powder and quartz powder, and the mica powder is commercially available phlogopite or muscovite. When used, it is ground to a particle size of 200-10000 mesh, preferably 800-2500 mesh, and existing grinding methods such as high-speed mechanical crushing, ball milling or air flow milling can be used.

[0011] The long-chain fatty acid powder used in the present invention is a mixed powder of one or more of palmitic acid, stearic acid, stearate, isostearic acid, eicosanoic acid, and behenic acid. When used, it is ground to a particle size of 200-2000 mesh, preferably 200-500 mesh; similarly, existing grinding methods such as high-speed mechanical crushing, ball milling or air flow milling can be used.

[0012] The nano silicon dioxide used in the present invention is commercially available nano silicon dioxide or hydrophobic nano silicon dioxide.

[0013] The low speed in the preparation method of the present invention is 300 r / min-350 r / min, and the high speed is 1200 r / min-1500 r / min.

[0014] The invention can be prepared by using a closed agitator with a temperature control function.

[0015] The advantages of the present invention are: innovative use of a melting method for super-hydrophobic modification, the method is simple, environmentally friendly, low in production cost, and easy to operate; the obtained finished powder is added to cement mortar as an additive, which can greatly improve the compression and wear resistance of the cement mortar and has good hydrophobic properties.

[0016] Its advantages are specifically reflected in the following points:

[0017] 1. Among the mineral admixture powders used in the present invention, mica powder is a natural flaky material with good toughness and properties such as high temperature resistance, corrosion resistance, and strong adhesion. As the base material of super-hydrophobic powder, it is easier to form a hydrophobic barrier and enhance the super-hydrophobic effect; the main component of corundum powder is the α phase of aluminum oxide, which not only has a layered structure, but also has high strength and wear resistance; quartz powder is a hard, wear-resistant, and chemically stable silicate mineral; all three are good base materials, which can give super-hydrophobic powder the properties of high strength and wear resistance.

[0018] Figure 1 Schematic diagram of the hydrophobic effect of super hydrophobic mica powder and corundum powder obtained after crushing according to the method of the present invention, Figure 2 This is the Fourier infrared spectrum of super hydrophobic mica powder. Figure 2 It can be seen that stearic acid and zinc stearate are closely combined with mica powder, mainly through physical modification, so that the mica powder achieves a super hydrophobic effect.

[0019] 2. Long-chain fatty acids are widely present in nature, low in cost, easy to obtain and naturally degrade. As hydrophobic modifiers, they are more environmentally friendly and green than hydrophobic agents such as siloxane and fluorosilane. At the same time, the melting points of long-chain fatty acids are mostly around 100 o C or less, this characteristic enables the powder to be heated to simultaneously construct a rough micro-nano structure and hydrophobically modified, and the two necessary conditions for super-hydrophobic modification can be met in one step. Since the present invention innovatively uses a melting method to perform super-hydrophobic modification on the mineral admixture powder, it fully utilizes the characteristics of heating and melting of long-chain fatty acids and cooling and hardening, and can perform super-hydrophobic modification on the powder more uniformly and stably, and has an enhancing effect on the hardness of the powder after cooling and solidification. The method is simple and efficient, and is easy to operate and mass-produce.

[0020] 3. Crushing and refining the mineral admixtures can expose more surface hydroxyl groups, which is beneficial to the occurrence of grafting reaction and convenient for hydrophobic modification; crushing and refining the long-chain fatty acids can make them more evenly distributed around the substrate and nano-silica, which is convenient for the formation of micro-nano structure and hydrophobic modification after melting, and improves the homogeneity and hydrophobic effect of super-hydrophobic powder.

[0021] 4. The hydroxyl groups on the surface of mineral micropowders can undergo an acid-base neutralization reaction with long-chain fatty acids to perform the first layer of hydrophobic modification. There are a large number of hydrogen bonds between the hydroxyl groups and the carboxyl groups, which can be used as the second layer of hydrophobic modification. The molten long-chain fatty acids are evenly coated on the surface of the micro- and nano-powders to play a bridging role. After cooling and solidification, the third layer of hydrophobic modification is formed. The multi-layer physical and chemical hydrophobic modification, the high-strength wear-resistant properties of the selected mineral micropowders and the constructed rough micro-nano structure form a high-performance, highly stable super-hydrophobic powder with better adaptability. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the hydrophobic effect of super hydrophobic mica powder and corundum powder obtained according to the method of the present invention.

[0023] Figure 2 This is the Fourier infrared spectrum of superhydrophobic mica powder.

[0024] Figure 3 The microstructure of the super-hydrophobic powder prepared in Example 1 under a scanning electron microscope.

[0025] Figure 4 is the contact angle of the super hydrophobic powder prepared in Example 1 applied on the glass surface. DETAILED DESCRIPTION

[0026] The method of the present invention is described in more detail below in conjunction with specific embodiments to facilitate understanding by those skilled in the art.

[0027] Example 1 Preparation of 1# high-strength wear-resistant super-hydrophobic powder

[0028] 500 g of muscovite was put into a planetary ball mill and crushed to 1000 mesh; 200 g of solid palmitic acid was crushed to 300 mesh by an ultrafine grinder;

[0029] Then, 500 g of crushed muscovite powder and 200 g of palmitic acid powder were added into a temperature-controlled closed mixer and stirred at a speed of 350 r / min.

[0030] After stopping stirring, raise the temperature in the stirring chamber to 90 o C, then increase the speed to 1200 r / min and continue stirring for 15 min;

[0031] Add 200 g of hydrophobic nano-silica into the stirrer, continue stirring for another 10 min, then stop heating and cool the powder to room temperature while stirring (still maintaining a speed of 1200 r / min);

[0032] Turn off stirring and take out the powder. o C for 4 h, and finally ground to about 800 mesh to obtain 1# high-strength, wear-resistant and super-hydrophobic powder product.

[0033] Figure 3 This is the microstructure of the finished product of 1# high-strength wear-resistant super-hydrophobic powder under a scanning electron microscope at different magnifications. It can be seen from the figure that nano-silicon dioxide is coated on the surface of mica powder to form a rough structure at the nanoscale. Figure 4 It is the contact angle of 1# superhydrophobic powder coated on the glass surface. It can be seen from the figure that the contact angle of the prepared 1# superhydrophobic powder is 153.1°, reaching a superhydrophobic state.

[0034] The prepared 1# super hydrophobic powder was added to cement mortar at a mass fraction of 5% to prepare hydrophobic mortar. The 28-day compressive strength of the prepared mortar specimen (70.7 mm×70.7 mm×70.7 mm) was 43.2 MPa, while that of the comparison specimen without hydrophobic powder was 38.12 MPa, that is, the high-strength wear-resistant super hydrophobic powder prepared by the present invention increased the compressive strength of the mortar by 13.3%. At the same time, the hydrophobic mortar prepared with 1# powder has excellent wear resistance. After the mortar reagent is polished with a flat polisher, the water contact angle reaches 151.1 o , that is, the hydrophobic mortar can still maintain good superhydrophobic properties.

[0035] Example 2 Preparation of 2# high-strength wear-resistant super-hydrophobic powder

[0036] 400 g of corundum powder was put into a planetary ball mill for crushing to 1200 mesh, and 300 g of solid stearic acid was crushed to 400 mesh by an ultrafine grinder;

[0037] Then, 400 g of the crushed corundum micropowder and 300 g of stearic acid micropowder were added into a temperature-controlled closed mixer in sequence, and stirred evenly at a speed of 300 r / min;

[0038] After stopping stirring, raise the temperature in the stirring chamber to 100 o C, then increase the speed to 1500 r / min and continue stirring for 10 min;

[0039] 300 g of hydrophobic nano-silicon dioxide was added to the stirrer, and the heating was stopped after stirring for 13 min. The powder was cooled to room temperature under stirring conditions (stirring speed was the same as in Example 1);

[0040] Turn off stirring and take out the powder. o C for 4 h, and finally ground to about 1000 mesh to obtain 2# high-strength, wear-resistant and super-hydrophobic powder product.

[0041] The prepared 2# powder was added into cement mortar at a dosage of 3% by mass to prepare hydrophobic mortar. The 28 d compressive strength of the prepared mortar specimens (same size as in Example 1) was 43.64 MPa, while that of the control specimens without hydrophobic powder was 37.14 MPa. The 2# high-strength, wear-resistant and super-hydrophobic powder increased the compressive strength of the mortar by 17.5%.

[0042] The mortar specimen was placed on sandpaper (sandpaper fineness 320 mesh), with a weight of 200 g pressed on the upper surface. The mortar specimen was pushed on the sandpaper and rubbed horizontally along the ruler for 200 mm, and then the specimen was pushed in the opposite direction and rubbed for 200 mm. This was one friction cycle. After repeating the friction cycle for 5 times, the water contact angle could still reach 150 o .

[0043] Example 3 Preparation of 3# high-strength wear-resistant super-hydrophobic powder

[0044] 250 g of muscovite and 200 g of corundum powder were put into a planetary ball mill for crushing to 800 mesh, and 200 g of stearic acid and 50 g of zinc stearate were crushed to 300 mesh by an ultrafine grinder;

[0045] Then, the crushed muscovite and corundum powder (450 g in total), stearic acid and zinc stearate powder (250 g in total) were added into a temperature-controlled closed mixer in sequence, and stirred evenly at a speed of 350 r / min;

[0046] After stopping stirring, raise the temperature in the stirring chamber to 140 o C, then increase the speed to 1500 r / min and continue stirring for 20 min;

[0047] 100 g of nano-silicon dioxide was added to the stirrer, and the heating was stopped after stirring for 16 min. The powder was cooled to room temperature under stirring conditions (stirring speed was the same as in Example 1);

[0048] Turn off stirring and take out the powder. o C for 4 h, and finally ground to about 800 mesh to obtain 3# high-strength, wear-resistant and super-hydrophobic powder product.

[0049] The 3# high-strength wear-resistant super-hydrophobic powder was added to cement mortar at a mass fraction of 6% to prepare a hydrophobic mortar. The prepared hydrophobic mortar was applied on the roughened concrete surface, which made the concrete surface super-hydrophobic and the contact angle could reach 155 o .

Claims

1. A method for preparing a high-strength wear-resistant super-hydrophobic powder, Features: It is prepared by melting method with raw material mineral admixture powder, nano silicon dioxide and long chain fatty acid powder in the following weight proportions: Proportion: 40-70 parts of mineral admixture powder, 10-50 parts of nano-silicon dioxide, and 5-30 parts of long-chain fatty acid powder; wherein the mineral admixture powder is one or two of mica powder and corundum powder, and the particle size thereof is 200-10000 mesh; the long-chain fatty acid powder is a mixed powder of one or more of palmitic acid, stearic acid, stearate, isostearic acid, eicosanoic acid, and behenic acid, and the particle size thereof is 200-2000 mesh; Preparation method: The mineral admixture and long-chain fatty acid are accurately weighed according to the above weight parts and put into a stirrer and stir evenly at a low speed, then gradually heat up to 80~160 ℃, maintain the temperature and stir at high speed for 10~30 min, then add the weighed nano-silicon dioxide, continue to stir at high speed for 10~20 min and then stop heating, cool the powder to room temperature under stirring conditions, then perform vacuum drying, and finally grind to obtain a high-strength, wear-resistant and super-hydrophobic powder product.

2. The method for preparing the high-strength wear-resistant super-hydrophobic powder according to claim 1, Features: The particle size of the mineral admixture powder is 800-2500 meshes.

3. The method for preparing the high-strength wear-resistant super-hydrophobic powder according to claim 1, Features: The particle size of the long-chain fatty acid powder is 200-500 meshes.

4. The method for preparing the high-strength wear-resistant super-hydrophobic powder according to claim 1, Features: The low speed in the preparation method is 300 r / min-350 r / min, and the high speed is 1200 r / min-1500 r / min.

Citation Information

Patent Citations

  • Inorganic substance super-hydrophobic paint and application thereof

    CN104672962A

  • A method for superhydrophobic modification of mineral admixtures

    CN108424020B

  • Nano modified inorganic mineral waterproof agent as well as preparation method and application thereof

    CN114163159A