Preparation and use method of ceramic self-cleaning coating
By using waste and nano titanium dioxide powder to prepare ceramic self-cleaning coatings, the existing ceramic self-cleaning coatings have solved the problems of complex process, high cost and unstable adhesion of existing ceramic self-cleaning coatings, and simple, low-cost and efficient preparation of ceramic self-cleaning coatings is achieved. Suitable for a variety of ceramic products.
Patent Information
- Application Number
- CN202310472781.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The preparation process of existing ceramic self-cleaning coatings is complex, has high cost, unstable coating adhesion, no sintering, and uneven thickness, which affects the self-cleaning effect.
The ceramic self-cleaning coating is prepared using waste such as alkali slag and boiling furnace slag, and nanotitanium dioxide powder is added, and it is evenly sonicated and stirred, and then brushed on the ceramic surface, and is maintained in the carbonization reactor to enhance adhesion and self-cleaning performance.
It realizes ceramic self-cleaning coatings with simple preparation technology, low cost, strong coating adhesion, uniform thickness and good self-cleaning effect, and is suitable for different types of ceramic products.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ceramic materials, and in particular relates to a preparation method of a ceramic self-cleaning coating and a use method thereof. Background Art
[0002] Ceramics is a common building material with good wear resistance, corrosion resistance, high temperature resistance and other properties. It is widely used in construction, home furnishing, kitchenware, bathroom and other fields. However, the surface of ceramics easily absorbs dirt, oil stains, etc., which is difficult to clean, affecting its appearance and hygiene. Therefore, the development of a ceramic self-cleaning coating that can form a self-cleaning effect on the ceramic surface has important application value.
[0003] The patent application with publication number CN107473714A discloses a UV self-cleaning ceramic and its preparation method. The preparation process is divided into several links, such as proportioning, ball milling, grouting, embryo repair and firing. First, various raw materials are mixed according to the proportion, ball milled with grinding balls to obtain porcelain mud, and then the porcelain mud is grouted and embryo repaired, fired at 400~500℃ for 1~2 hours, then stayed at 700~900℃ for 2~3 hours, and finally heated to 1250~1350℃, fired for 1~2 hours to make UV self-cleaning ceramic. This product has the effect of UV self-cleaning, and can be used in combination with UV lamps to make efficient and clean toilet products.
[0004] The patent application with publication number CN111204977A discloses a ceramic glaze with self-cleaning nano-cure and easy-to-clean properties and its preparation method. The glaze is composed of a variety of raw materials, including ceramic glaze, glass, boric acid powder, calcite, kaolin, Sanbaopeng porcelain stone, Qimen porcelain stone, quartz, magnesium carbonate, dolomite and barium carbonate. After firing, the ceramic surface presents a smooth and bright surface, is not easily stained, and has good self-cleaning function.
[0005] The patent application with publication number CN111087835A discloses a method for preparing a nano self-cleaning environmentally friendly coating. First, a nano titanium dioxide colloidal substance is added to a stirred reactor, and a certain amount of deionized water, ethanol and an organic solvent are added to react to obtain a nano titanium dioxide colloidal solution. Then the nano titanium dioxide colloidal solution is added to a heated stirrer, and materials such as zeolite, inorganic environmentally friendly filler, polyvinyl pyrrolidone and sodium benzoate are added to react to obtain a nano titanium dioxide emulsion. Finally, a thickener and a defoamer are added to the nano titanium dioxide emulsion to prepare a nano self-cleaning environmentally friendly coating. The coating has super hydrophobic and oleophobic properties and excellent self-cleaning properties. In addition, the invention also provides a ball milling device for grinding and refining titanium dioxide particles, which can be used in a mixed material for ball milling to achieve a better effect.
[0006] At present, some studies have reported on the preparation methods of self-cleaning ceramics. Among them, the method of using the synergistic effect of the photocatalytic degradation reaction of surface stains on the surface of TiO2 ceramics under light conditions and the rinsing of the super-hydrophilicity of TiO2 to produce a self-cleaning effect is a relatively effective method. However, the existing self-cleaning ceramics have the following problems: the preparation process is complicated and the cost is high; the self-cleaning coating needs to be sintered, which affects the activity of TiO2; the adhesion of the self-cleaning coating is unstable and easy to fall off; the thickness of the self-cleaning coating is uneven, which affects the self-cleaning effect. Therefore, it is necessary to provide a ceramic self-cleaning coating with a simple preparation process, low cost, strong coating adhesion, no need for sintering, uniform coating thickness, and good self-cleaning effect. Summary of the invention
[0007] The purpose of the present invention is to provide a ceramic self-cleaning coating with simple preparation process, low cost, no sintering required, strong coating adhesion, uniform coating thickness and good self-cleaning effect, and a use method thereof.
[0008] To achieve the above object, the present invention provides the following technical solutions:
[0009] 1) According to the weight ratio, 31-78 parts of alkaline slag and 20-35 parts of boiling furnace slag are mixed evenly, fired at 1200-1300°C for 1.5-2.5 hours, and cooled in the furnace to obtain mixture A.
[0010] 2) According to the weight proportions, 31-78 parts of alkaline slag, 20-35 parts of boiling furnace slag and 1-2 parts of sintering aid are mixed evenly, fired at 1200-1300°C for 1.5-2.5 hours, and cooled in the furnace to obtain mixture B.
[0011] 3) According to the weight ratio, 14 to 20 parts of nano titanium dioxide powder and the rest of deionized water are dispersed in water and ultrasonically treated until a uniform nano titanium dioxide suspension is obtained.
[0012] 4) According to the weight percentage, 15-25 parts of mixture A and 45-75 parts of mixture B are added to the nano titanium dioxide suspension and stirred evenly to obtain a ceramic self-cleaning coating.
[0013] 5) The prepared self-cleaning coating is applied to the surface of the ceramic body by brushing.
[0014] 6) The ceramic body coated with the self-cleaning coating is placed in a carbonization reactor for curing so that the self-cleaning coating is tightly bonded to the body.
[0015] Preferably, the stirring addition sequence is: first, pour the nano titanium dioxide suspension into the stirring container, then add the mixture A and the mixture B into the stirring container respectively, and stir;
[0016] Stirring speed: 300-500 rpm to ensure that the components are thoroughly mixed while preventing the generation of bubbles due to excessive stirring.
[0017] Stirring time: The total stirring time is 15 to 30 minutes.
[0018] Preferably, the carbonization curing reaction is carried out by introducing CO2 into the carbonization reactor at a rate of 0.5 to 2 L / min under normal pressure conditions, and the carbonization time is 1 to 3 h.
[0019] Compared with the prior art, the advantages and beneficial effects of the present invention are:
[0020] 1. Preparation of ceramic self-cleaning coatings using waste: Ceramic self-cleaning coatings are prepared by using waste such as alkali slag and boiling furnace slag. The method of waste resource utilization is used to prepare ceramic self-cleaning coatings, which is low-cost, environmentally friendly and energy-saving.
[0021] 2. Introducing nano-titanium dioxide powder during the preparation process: Nano-titanium dioxide has good photocatalytic function, can decompose organic matter, and has a self-cleaning effect. After the introduction of nano-titanium dioxide, the ceramic self-cleaning coating has strong photocatalytic activity and self-cleaning performance.
[0022] 3. Simple usage: Use a simple brushing method to apply the self-cleaning coating to the surface of the ceramic body. The specific process parameters are clear and the operation is simple.
[0023] 4. Wide application scenarios: This ceramic self-cleaning coating is suitable for different types of ceramic products, such as sanitary ware, tiles, tableware, etc., and has wide market application potential. DETAILED DESCRIPTION
[0024] The embodiments of the present invention further illustrate the technical solution. These embodiments are only part of the present invention. Without creative work by technicians in the relevant fields, all other embodiments also belong to the protection scope of the present invention.
[0025] Example 1
[0026] Step 1: Calculate by weight, put 32 parts of alkali slag and 20 parts of boiling furnace slag into a ball mill for 2 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, and then sinter it at a high temperature of 1250°C in a tube furnace and keep it warm for 2 hours. After cooling with the furnace, mixture A is obtained.
[0027] Step 2: Calculate by weight, put 30 parts of alkali slag, 19 parts of boiling furnace slag and 1.5 parts of sintering aid into a ball mill for 2 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, and then sinter it at a high temperature of 1250°C in a tubular furnace and keep it warm for 2 hours. After cooling with the furnace, mixture B is obtained.
[0028] Step 3: Mix 15 parts of nano titanium dioxide powder and the rest of deionized water and mix them evenly, then use an ultrasonic processor to perform ultrasonic treatment again to make it more evenly dispersed in water, so as to prepare a nano titanium dioxide suspension.
[0029] Step 4: According to the weight percentage, gradually add 120 parts of mixture B and 50 parts of mixture A to the nano titanium dioxide suspension. Stir while adding, and use machine stirring or manual stirring to stir the mixture evenly until all the materials are evenly mixed together.
[0030] Step 5: Clean the surface of the ceramic body and ensure that the surface is dry, smooth, and free of impurities such as oil and dust; first stir the self-cleaning paint evenly and pour it into a clean container, then dip an appropriate amount of paint and start to apply it smoothly on the surface of the ceramic body from one direction; the brush should be perpendicular to the flow direction of the paint to ensure that the paint is evenly covered on the surface; use a short-bristled brush with a bristle length of 2.5 cm to facilitate the control of paint thickness and avoid missing brushes and sagging; and pay attention to accurate construction, carefully observe each area, and check whether there are any uncovered areas or too full areas and repeat the painting twice.
[0031] Step 6: Place the ceramic blank coated with the self-cleaning coating into a carbonization reactor for curing. The carbonization procedure is set as follows:
[0032] S1. Carbonization rate: CO2 was introduced at a rate of 1.5 L / min under normal pressure.
[0033] S2. Carbonization time: 3 hours.
[0034] Example 2
[0035] Step 1: Calculate by weight, put 50 parts of alkali slag and 25 parts of boiling furnace slag into a ball mill for 3 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, then sinter it at a high temperature of 1300°C in a tube furnace and keep it warm for 2 hours. After cooling with the furnace, mixture A is obtained.
[0036] Step 2: Calculate by weight, put 54 parts of alkali residue, 24 parts of boiling furnace slag and 1 part of sintering aid into a ball mill for 2.5 hours of ball milling, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, and then sinter it at a high temperature of 1250°C in a tubular furnace and keep it warm for 2 hours. After cooling with the furnace, mixture B is obtained.
[0037] Step 3: Mix 18 parts of nano titanium dioxide powder and the rest of deionized water and mix them evenly, then use an ultrasonic processor to perform ultrasonic treatment again to make it more evenly dispersed in water, so as to prepare a nano titanium dioxide suspension.
[0038] Step 4: According to the weight percentage, gradually add 20 parts of mixture B and 73 parts of mixture A to the nano titanium dioxide suspension. Stir while adding, and use machine stirring or manual stirring to stir the mixture evenly until all the materials are evenly mixed together.
[0039] Step 5: Clean the surface of the ceramic body and ensure that the surface is dry, smooth, and free of impurities such as oil and dust; first stir the self-cleaning paint evenly and pour it into a clean container, then dip an appropriate amount of paint and start to apply it smoothly on the surface of the ceramic body from one direction; the brush should be directed perpendicular to the flow direction of the paint to ensure that the paint is evenly covered on the surface; use a short-bristled brush with a bristle length of 2.5 cm to facilitate the control of paint thickness and avoid missing brushes and sagging; and pay attention to accurate construction, carefully observe each area, and check whether there are any uncovered areas or too full areas and repeat the painting twice.
[0040] Step 6: Place the ceramic blank coated with the self-cleaning coating into a carbonization reactor for curing. The carbonization procedure is set as follows:
[0041] S1. Carbonization rate: CO2 was introduced at a rate of 1 L / min under normal pressure.
[0042] S2. Carbonization time: 2 hours.
[0043] Example 3
[0044] Step 1: Calculate by weight, put 75 parts of alkali slag and 22 parts of boiling furnace slag into a ball mill for 1.5 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, and then sinter it at a high temperature of 1250°C in a tube furnace and keep it warm for 2 hours. After cooling with the furnace, mixture A is obtained.
[0045] Step 2: Calculate by weight, put 70 parts of alkali slag, 22 parts of boiling furnace slag and 1.5 parts of sintering aid into a ball mill for 2 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, and then sinter it at a high temperature of 1250°C in a tube furnace and keep it warm for 2 hours. After cooling with the furnace, mixture B is obtained.
[0046] Step 3: Mix 17 parts of nano titanium dioxide powder and the rest of deionized water and mix them evenly, then use an ultrasonic processor to perform ultrasonic treatment again to make it more evenly dispersed in water, so as to prepare a nano titanium dioxide suspension.
[0047] Step 4: According to the weight percentage, gradually add 20 parts of mixture B and 75 parts of mixture A to the nano titanium dioxide suspension. Stir while adding, and you can use machine stirring or manual stirring to stir the mixture evenly until all the materials are evenly mixed together.
[0048] Step 5: Clean the surface of the ceramic body and ensure that the surface is dry, smooth, and free of impurities such as oil and dust; first stir the self-cleaning paint evenly and pour it into a clean container, then dip an appropriate amount of paint and start to apply it smoothly on the surface of the ceramic body from one direction; the brush should be directed perpendicular to the flow direction of the paint to ensure that the paint is evenly covered on the surface; use a short-bristled brush with a bristle length of 2.5 cm to facilitate the control of paint thickness and avoid missing brushes and sagging; and pay attention to accurate construction, carefully observe each area, and check whether there are any uncovered areas or too full areas and repeat the painting twice.
[0049] Step 6: Place the ceramic blank coated with the self-cleaning coating into a carbonization reactor for curing. The carbonization procedure is set as follows:
[0050] S1. Carbonization rate: CO2 was introduced at a rate of 2 L / min under normal pressure.
[0051] S2. Carbonization time: 1 hour.
[0052] Example 4
[0053] Step 1: Calculate by weight, put 60 parts of alkali slag and 21 parts of boiling furnace slag into a ball mill for 2 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, then sinter it at a high temperature of 1300°C in a tube furnace and keep it warm for 2 hours. After cooling with the furnace, mixture B is obtained.
[0054] Step 2: Calculate by weight, put 70 parts of alkali slag, 22 parts of boiling furnace slag and 1.5 parts of sintering aid into a ball mill for 2 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, and then sinter it at a high temperature of 1300°C in a tubular furnace and keep it warm for 2 hours. After cooling in the furnace, Mixture B .
[0055] Step 3: Mix 14 to 20 parts of nano titanium dioxide powder and the rest of deionized water and mix them evenly, then use an ultrasonic processor to perform ultrasonic treatment again to make it more evenly dispersed in water, so as to prepare a nano titanium dioxide suspension.
[0056] Step 4: According to the weight percentage, gradually add 20 parts of mixture B and 70 parts of mixture A to the nano titanium dioxide suspension. Stir while adding, and use machine stirring or manual stirring to stir the mixture evenly until all the materials are evenly mixed together.
[0057] Step 5: Clean the surface of the ceramic body and ensure that the surface is dry, smooth, and free of impurities such as oil and dust; first stir the self-cleaning paint evenly and pour it into a clean container, then dip an appropriate amount of paint and start to apply it smoothly on the surface of the ceramic body from one direction; the brush should be directed perpendicular to the flow direction of the paint to ensure that the paint is evenly covered on the surface; use a short-bristled brush with a bristle length of 2.5 cm to facilitate the control of paint thickness and avoid missing brushes and sagging; and pay attention to accurate construction, carefully observe each area, and check whether there are any uncovered areas or too full areas and repeat the painting twice.
[0058] Step 6: Place the ceramic blank coated with the self-cleaning coating into a carbonization reactor for curing. The carbonization procedure is set as follows:
[0059] S1. Carbonization rate: CO2 was introduced at a rate of 1.5 L / min under normal pressure.
[0060] S2. Carbonization time: 2 hours.
[0061] Example 5
[0062] Step 1: Calculate by weight, put 75 parts of alkali slag and 24 parts of boiling furnace slag into a ball mill for 3 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, then sinter it at a high temperature of 1200°C in a tubular furnace and keep it warm for 1.5 hours. After cooling with the furnace, mixture A is obtained.
[0063] Step 2: Calculate by weight, put 276 parts of alkali residue, 18 parts of boiling furnace slag and 1 part of sintering aid into a ball mill for 3 hours, then add 10 parts of water to the dried mixture, mix well and pour into a mold. Apply a pressure of 8 MPa in the tablet press to press the mixture into a cylindrical tablet with a diameter of 3 cm. Put the cylindrical tablet into an alumina crucible, and then sinter it at a high temperature of 1300°C in a tube furnace and keep it warm for 2.5 hours. After cooling with the furnace, mixture B is obtained.
[0064] Step 3: Mix 20 parts of nano titanium dioxide powder and the rest of deionized water and mix them evenly, then use an ultrasonic processor to perform ultrasonic treatment again to make it more evenly dispersed in water, so as to prepare a nano titanium dioxide suspension.
[0065] Step 4: According to the weight percentage, gradually add 15 parts of mixture B and 75 parts of mixture A to the nano titanium dioxide suspension. Stir while adding, and you can use machine stirring or manual stirring to stir the mixture evenly until all the materials are evenly mixed together.
[0066] Step 5: Clean the surface of the ceramic body and ensure that the surface is dry, smooth, and free of impurities such as oil and dust; first stir the self-cleaning paint evenly and pour it into a clean container, then dip an appropriate amount of paint and start to apply it smoothly on the surface of the ceramic body from one direction; the brush should be directed perpendicular to the flow direction of the paint to ensure that the paint is evenly covered on the surface; use a short-bristled brush with a bristle length of 2.5 cm to facilitate the control of paint thickness and avoid missing brushes and sagging; and pay attention to accurate construction, carefully observe each area, and check whether there are any uncovered areas or too full areas and repeat the painting twice.
[0067] Step 6: Place the ceramic blank coated with the self-cleaning coating into a carbonization reactor for curing. The carbonization procedure is set as follows:
[0068] S1. Carbonization rate: CO2 was introduced at a rate of 0.5 L / min under normal pressure.
[0069] S2. Carbonization time: 3 hours.
[0070] Performance Test:
[0071] The following self-cleaning properties, wear resistance, and coating adhesion properties were tested. The main test methods are as follows:
[0072] (1) The self-cleaning test includes two aspects:
[0073] Degradation performance test: Dyes such as methylene blue or rhodamine B can be used for photodegradation experiments, and the effect of surface photocatalytic degradation of organic matter can be evaluated by detecting the disappearance rate or color reduction rate of the dye in the dye solution.
[0074] Super hydrophilicity test: The super hydrophilicity of a material can be evaluated by testing the contact angle of the surface. The contact angle of the sample surface is generally measured by titration or tilted plate method. The specific method and instrument can be determined according to the selected test standard.
[0075] The following specific test methods are used:
[0076] Photocatalytic performance test: First prepare a dye solution (such as methylene blue or rhodamine B), pour it into a container, and then place a certain amount of self-cleaning ceramic samples into the solution under a light source. Record the speed at which the dye disappears or the color reduction rate, and compare it with the control group without using self-cleaning ceramics.
[0077] Super hydrophilicity test: Use the titration method or tilted plate method to measure the contact angle of the sample. The specific steps are as follows:
[0078] Titration method: drop a drop of pure water on the ceramic surface, and slowly lift it up with a micro-syringe with adjustable height until the drop of water disappears from the ceramic surface. Record the droplet diameter and volume when it drops, and then calculate the contact angle. The specific formula is: cosθ = (h / r) × 2, where h is the droplet height and r is the droplet radius.
[0079] Inclined plate method: Place the self-cleaning ceramic sample on an adjustable slope inclined plate and slowly tilt the inclined plate until the water drop starts to flow. The contact angle is calculated from the angle of the water drop sliding down and the tilt angle. The specific formula is: cosθ = sinα / sinβ, where α is the angle of the water drop sliding down and β is the tilt angle.
[0080] (2) Wear resistance: Place the sample on the test machine bracket to ensure that the contact area between the sample and the test machine fixture is uniform and the clamping force is appropriate; conduct experimental tests: Use sliding method to measure the wear resistance of the ceramic self-cleaning coating to friction, use the universal testing machine to control the set load parameters, and perform load and removal operations on the sample. The detection goal is to ensure that the force required to destroy the coating is applied and record the experimental data; use the data provided by the universal testing machine to analyze the wear resistance and indirect wear value of the ceramic self-cleaning coating, directly quantitatively evaluate the performance of the coating from the data, and systematically measure its friction and wear resistance.
[0081] (2) Coating adhesion performance:
[0082] First, adjust the test parameters: standard load is 10N, speed is 20mm / s, and sliding distance is 40mm.
[0083] Test operation: Place the clean and dry self-cleaning ceramic specimen on the test bench; Set the test conditions, press the scraper in the test device to the surface of the specimen, and perform unidirectional scraping under the set load; After scraping, use a metal ruler to measure and record the length and number of each mark, and use a microscope to check and determine its type and depth; Repeat the above steps 3-4 times until satisfactory test data is obtained.
[0084] Record data and evaluate results. Perform statistics and analysis on the data recorded for each test, including average trace length, standard deviation, maximum trace length and other indicators.
[0085] Combining the above test methods, the performance indicators of the product are measured as shown in the following table:
[0086] Example performance indicators Color reduction rate Contact angle (°) Wear rate Scratch length (mm) Example 1 100% 8.265 0.05 4.56 Example 2 100% 7.256 0.06 3.46 Example 3 100% 8.596 0.05 3.24 Example 4 100% 6.158 0.05 4.87 Example 5 100% 6.258 0.06 4.63
[0087] The specific embodiments of the present invention have been described in detail above, but this is not a limitation of the present invention. Any technician can modify and improve the present invention based on the spirit and principles of the present invention, and these modifications and improvements should be considered within the scope of protection of the present invention.
Claims
1. A ceramic self-cleaning coating, characterized in that: The method comprises the following preparation steps: Step A: Calculate by weight, mix 31-78 parts of alkali slag and 20-35 parts of boiling furnace slag, and then sinter them to 1200-1300℃ for 1.5-2.5 hours, and then cool them down to obtain γ - a mixture A of Ca2SiO4, Ca3SiO5, CaAl2O4 and CaFeAlO4; Step B: Calculate by weight, mix 31-78 parts of alkali slag, 20-35 parts of boiling furnace slag and 1-2 parts of sintering aid, and then sinter to 1200-1300℃ for 1.5-2.5 hours, and then cool with the furnace to obtain β - a mixture B of Ca2SiO4, Ca3SiO5, CaAl2O4 and CaFeAlO4; Step C: taking 14 to 20 parts of nano titanium dioxide powder and the rest of deionized water according to weight, dispersing the nano titanium dioxide powder in the deionized water, and performing ultrasonic treatment until a uniform nano titanium dioxide suspension is obtained; Step D: According to the weight percentage, 15-25 parts of mixture A and 45-75 parts of mixture B are added to the nano titanium dioxide suspension and stirred evenly to obtain a ceramic self-cleaning coating.
2. A ceramic self-cleaning coating according to claim 1, characterized in that: The alkali residue is the alkali residue of the ammonia-alkali process alkali-making plant, and its main component is calcium carbonate with a content of 60-80%.
3. A ceramic self-cleaning coating according to claim 1, characterized in that: The boiling furnace slag is waste slag formed when coal gangue or coal is burned at high temperature in a boiling furnace, in which non-combustible silicon, aluminum and iron elements are enriched in the form of doping. The main effective component is silicon dioxide, with a content of 60-75%.
4. A ceramic self-cleaning coating according to claim 1, characterized in that: The sintering aid is bauxite waste slag, with an alumina content of more than 30% and a silicate content of 10-20%.
5. A ceramic self-cleaning coating according to claim 1, characterized in that: The particle size of the nano titanium dioxide powder is 5-50 nm, and the crystal shape is spherical or rod-shaped.
6. The method for using a ceramic self-cleaning coating according to claim 1, characterized in that: The method comprises the following preparation steps: step A: coating the prepared self-cleaning coating on the surface of a ceramic body by brushing; step B: placing the ceramic body coated with the self-cleaning coating in a carbonization reactor for curing, so that the self-cleaning coating is tightly combined with the body.
7. The method for using a ceramic self-cleaning coating according to claim 6, characterized in that: The specific process parameters of the brush coating method are: the length of the brush hair is 2 to 3 cm; the coating rate is 90 to 100 g / ㎡; and the coating thickness is 50 to 200 μm.
8. The method for using a ceramic self-cleaning coating according to claim 6, characterized in that: The carbonization method is atmospheric pressure carbonization, and the carbonization time is 1 to 3 hours.