A waterborne epoxy heavy-duty anticorrosive coating and preparation method thereof
By forming a scaly powder with a three-layer structure of ZnO/Zn/ZnO on the surface of metallic zinc and a ball milling + high-speed dispersion process, a water-based epoxy heavy-duty anti-corrosion coating is prepared, which solves the problems of short service life and environmental pollution of existing coatings and achieves Long-term anti-corrosion and low-treatment rust surface coating significantly improve the shielding performance and environmental friendliness of the coating.
Patent Information
- Application Number
- CN202310723997.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-06-19
AI Technical Summary
Existing heavy-duty anti-corrosion coatings have a short service life, cause great environmental pollution, and have high rust removal construction costs. It is difficult to achieve low-treatment rust surface coating, which affects the anti-corrosion effect of the coating.
Using scaly powder as filler, scaly particles with a three-layer structure of ZnO/Zn/ZnO are formed on the surface of metallic zinc, combined with ball milling and high-speed dispersion processes, to prepare water-based epoxy heavy-duty anti-corrosion coatings to form a conductive overall coating to improve anti-corrosion performance and reduce pre-processing requirements.
It achieves long-term anti-corrosion effect, reduces pre-treatment costs, improves the shielding performance and environmental friendliness of the coating, can directly coat rusty surfaces under low-treatment conditions, and significantly extends the service life of the coating.
Smart Images

Figure CN116554760B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material surface anticorrosion, and in particular to a waterborne epoxy heavy-duty anticorrosion coating and a preparation method thereof. Background Art
[0002] The coating is composed of high molecular polymers and fillers, etc., and is applied on the surface of the substrate to form a corrosion-resistant coating. The coating is used to cover the surface of steel to shield the steel and isolate the steel from contact with the corrosive medium to achieve the purpose of corrosion prevention. Adding metallic zinc powder as a filler to the high molecular polymer to form a zinc-rich coating is currently the most widely used anti-corrosion measure in China.
[0003] Zinc-rich paint is prepared by adding spherical powder. For spherical powder, its theoretical stacking fraction is 68%, and its porosity is 32%, and its shielding performance is poor. At the same time, when the volume of spherical particles is constant, the surface area is the smallest, which easily leads to the precipitation of filler particles, greatly reducing the coating effect of the paint. Flake powder as a filler represents the development direction of anti-corrosion coatings. Among them, glass flake mastic paint with flake glass as a filler is widely used.
[0004] The electrode potential of the rust on the surface of steel, that is, the oxide, is higher than that of pure iron. Due to the presence of oxides, it will form a primary cell with the iron of the substrate, produce an electrochemical reaction, and the iron of the substrate will be oxidized into oxides. At the same time, the oxide layer becomes thicker, thereby reducing the anti-corrosion effect of the coating. In order to ensure the anti-corrosion effect of the coating, the anti-corrosion coating must remove oil, dirt and rust from the surface of the substrate before construction, and the rust must be completely removed. Among them, rust removal work is not only environmentally harsh, but also its cost accounts for about 50% of the cost of the entire coating. In particular, for large and complex components, when the rust removal does not reach the Sa21 / 2 level specified in GB / T8923.1, the anti-corrosion effect of the coating is significantly reduced, which seriously increases the anti-corrosion cost of equipment and facilities and reduces their service life. It is a general trend to reduce the requirements for pre-treatment and achieve low-treatment and rust-surface coating.
[0005] In addition, water-based paint reduces the pollution of the atmosphere and environment caused by the volatilization of organic matter, improves the construction working environment, represents the direction of paint development, and is environmentally friendly. Summary of the invention
[0006] The purpose of the present invention is to address the problems of service life, environmental protection and rust removal construction of existing heavy-duty anti-corrosion coatings, and to construct the anti-corrosion performance of water-based heavy-duty anti-corrosion coatings based on flaky powders as fillers to achieve a long-term anti-corrosion effect.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is:
[0008] A waterborne epoxy heavy-duty anticorrosive coating, comprising a filler-curing agent component and a resin component, wherein the resin component is an epoxy resin solution, the filler-curing agent component is composed of flaky powder, a curing agent solution, a dispersant and a solvent, the flaky powder is a ZnO / Zn / ZnO three-layer structure flaky particle formed by in-situ forming a ZnO layer with a thickness of 0.1 to 20 nm on the surface of metal Zn, and the D 50 In the range of 2 to 25 μm, the thickness is less than 0.1 μm;
[0009] The zinc oxide layer formed on the zinc surface is a dense film that prevents zinc from further oxidation. The zinc oxide film has transparent conductivity, a wide bandgap and a stable phase structure. The main functions of this three-layer structure design are: reducing the corrosion rate of the shielding layer formed by the filler itself, maintaining the anti-corrosion and cathodic protection functions of metallic zinc as a filler, and preventing zinc from reacting with solvents to precipitate gas during preparation and storage.
[0010] The filler-curing agent component and the resin component are mixed evenly before coating, and the weight ratio of the flaky powder in the dry coating formed after coating the substrate surface is greater than 90%. The flaky powder in the coating is alternately stacked in the form of layers to form the organizational structure of the anti-corrosion coating. The scales are conductive, and the coating forms a conductive whole.
[0011] The method for preparing the flaky powder used in the present invention is as follows: 50 Zn powder in the range of 5 to 50 μm is used as raw material and ball milled in a ball mill with a material: ball: water ratio of 1:1.5:0.8. The ball milling time directly determines the thickness of the zinc oxide layer and is strictly controlled within 1 to 4 hours. In order to prevent the formation of zinc hydroxide, the powder after ball milling is kept at 250°C for 1 to 2 hours to convert all zinc hydroxide into zinc oxide.
[0012] As a preferred technical solution of the present invention, in the filler-curing agent component, the weight ratio of flaky powder, curing agent solution, dispersant and solvent is 160-180:4.5-5.5:1-1.5:50-100, and the epoxy resin in the resin component is added based on the weight ratio of flaky powder in the dry coating being greater than 90%.
[0013] According to the two-dimensional characteristics of the flaky metal powder, the present invention is matched with a coating ratio and a process to achieve low-treatment rust or non-rust coating of the surface of the steel material by the coating, thereby achieving a long-term anti-corrosion effect.
[0014] In terms of coating proportion, the weight ratio of flaky powder filler in the formed coating is greater than 90%. The size control of flaky powder particles is a prerequisite. Only when the thickness of flaky particles is less than 0.1μm, D 50When the particle size is in the range of 2 to 25 μm, the particles always remain flat and suspended in the liquid to obtain the required coating structure.
[0015] The flaky powder particles exist as agglomerates formed by contact between two-dimensional planes. Separating the flaky particles to form a highly dispersed body is the key to preparing high-performance anti-corrosion coatings. Based on numerous experiments, the present invention summarizes the slurry preparation process of ball milling + high-speed dispersion to achieve uniform distribution of flaky powders.
[0016] A thixotropic fluid method is proposed for the stability of the slurry to ensure the stability of the slurry during storage. In theory, all slurries tend to precipitate, especially the slurry system of the present invention, where the amount of powder added is as high as more than 90%, and the resin content is low. The density of the powder particles is greatly different from that of the solvent. Once precipitation occurs, scales will be formed and agglomerated with each other, deteriorating the performance of the coating.
[0017] For this purpose, the thixotropic fluid method is adopted, and the slurry after high-speed dispersion becomes a thixotropic fluid, ensuring that the coating does not precipitate during storage and placement. That is, the coating exhibits solid characteristics and gel state when no force is applied, and exhibits sol state when stirred and subjected to force, with good viscosity and fluidity, while improving the sag properties during the coating process.
[0018] The preparation method of the waterborne epoxy heavy-duty anticorrosive coating proposed by the present invention comprises the following steps:
[0019] (1) Ball milling
[0020] The flaky powder, curing agent solution, dispersant and solvent are added into a ball mill and ground for 4 to 6 hours, and no water is contained in the ball milling process;
[0021] (2) High-speed dispersion
[0022] Pour the ball-milled slurry into a high-speed disperser and disperse it for 0.5 to 2 hours at a line speed greater than 50 m / s;
[0023] (3) Slurry
[0024] The dispersed slurry is poured out and placed in a container to obtain a filler-curing agent component; the dispersed slurry forms a thixotropic fluid, that is, the slurry becomes gel-like when not subjected to force, showing solid properties, and once subjected to force, that is, when stirred, it immediately forms a slurry, showing sol properties, and undergoes a reversible transformation between gel and sol, ensuring that the coating does not precipitate during storage;
[0025] (4) Preparation of resin component
[0026] Add epoxy resin and water into a container, and stir at 5 to 35° C. for 10 to 30 minutes to obtain a resin component;
[0027] (5) Preparation of coating
[0028] The prepared filler-curing agent component and resin component are mixed evenly to obtain a water-based epoxy heavy-duty anti-corrosion coating.
[0029] According to the requirements of heavy-duty anti-corrosion coatings, the present invention designs flaky powders of ZnO / Zn / ZnO structure as fillers, which not only fully utilizes the anti-corrosion characteristics of metal zinc as fillers, but also suppresses the corrosion rate of metal zinc to the greatest extent, and is equipped with a preparation process of ball milling + high-speed dispersion to achieve a long-term anti-corrosion effect. Compared with the prior art, the present invention has the following beneficial effects:
[0030] 1. Excellent anti-corrosion performance. The ultra-fine flaky powder of a specific size used in the present invention is used as a filler. On the one hand, the flaky powder itself has excellent anti-corrosion performance. The powder used is a three-layer structure of ZnO / Zn / ZnO, and a dense zinc oxide layer is formed in situ on the surface of the metal zinc. Zinc oxide has excellent anti-corrosion performance in marine and atmospheric environments, preventing the medium from reacting with the internal metal zinc and playing a shielding role. Compared with pure metal zinc as a filler, the anti-corrosion performance of the filler itself is improved, and the shielding performance of the coating is improved. On the other hand, the flaky powder is arranged in sheets in the coating, and one dimension of its three-dimensional size is at the submicron or nanometer level, and the other two dimensions are at the micron level. Such a special planar structure not only maintains the good dispersibility of the micron-level powder, but also enables it to exert the functional characteristics of the nano powder, with high surface activity and effective combination with other active groups. Therefore, the coating is dense, has a significant shielding effect, and is more densely attached to the surface of the metal substrate, thereby obtaining excellent anti-rust and anti-corrosion performance.
[0031] In addition, the content of flaky powder filler in the formed coating is greater than 90%, the thickness of the scales is less than 0.1μm, the thickness of the ZnO layer is less than 20nm, and a tunnel effect is generated between the scales to cause conduction (a thin insulating layer is sandwiched between two layers of metal conductors to form an electron tunnel junction. Experiments have found that electrons can pass through the tunnel junction, that is, electrons can pass through the insulating layer, which is the tunnel effect), and the coating forms a conductive whole and has a cathodic protection function.
[0032] 2. Environmental friendliness. The coating prepared by the present invention is a water-based coating, which uses water as a solvent to partially replace traditional organic solvents, thereby reducing the emission of harmful gases and being more friendly to the ecological environment.
[0033] 3. Low pre-treatment requirements. It can be directly filled with rusty surfaces for painting, thereby reducing the requirements for pre-treatment, improving the painting environment, and reducing the cost of painting. In this coating, flaky powder is used as a filler, and the layers are arranged in a plane, and the coating forms a conductive whole, which makes active rust inert and solid, making rust surface painting possible. It can greatly improve the film bonding strength of the coating, and can be directly painted on the substrate surface after removing oil, dirt, and floating rust (floating rust refers to a rust layer with poor bonding to the substrate surface and is very easy to fall off, while the rust layer with strong bonding to the substrate under the floating rust does not need to be removed). The traditional pre-treatment must be Sa2.5, while the coating pre-treatment of the present invention is St2, which organically unifies the convenience of painting and long-term corrosion protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 Schematic diagram of the structure (a) and coating (b) of the flaky powder prepared by the present invention.
[0035] Figure 2 These are SEM and XRD images of the flaky powder prepared by the present invention.
[0036] Figure 3 The present invention shows the surface morphology of the coating after being subjected to a 4000-hour salt spray test.
[0037] Figure 4 is the polarization curve of the coating prepared by the present invention. DETAILED DESCRIPTION
[0038] Example 1
[0039] The raw materials used in this embodiment are from:
[0040] Zn powder, D 50 In the range of 5 to 50 μm.
[0041] The curing agent solution was purchased from Shandong Ruisan Chemical Technology Co., Ltd., in which the solvent component accounted for about 30-50%.
[0042] The solvent propylene glycol methyl ether was purchased from Wuxi Yatai United Chemical Co., Ltd.
[0043] Dispersant was purchased from Nanjing Tianxing New Materials Co., Ltd.
[0044] The epoxy resin solution was purchased from Shandong Ruisan Chemical Technology Co., Ltd., in which water accounted for about 30-50%.
[0045] The method for preparing a waterborne epoxy heavy-duty anticorrosive coating in this embodiment comprises the following specific steps:
[0046] (1) Preparation of flaky powder
[0047] Zn powder was selected as raw material and ball milled in a ball mill with a material: ball: water ratio of 1:1.5:0.8; the ball milling time was 3.5 hours, and the ball-milled powder was kept at 250°C for 2 hours to obtain flaky powder.
[0048] The flaky powder structure prepared in this example Figure 1 As shown in a, it is a three-layer structure of ZnO / Zn / ZnO formed by in-situ formation of a ZnO layer on the surface of metal Zn. The flaky powder in the prepared coating is alternately stacked in the form of layers to form the organizational structure of the anti-corrosion coating. The scales are connected, and the coating forms a conductive whole ( Figure 1 b).
[0049] Figure 2 The SEM and XRD images of the flaky powder prepared by the present invention are shown in FIG. Figure 2 a and b correspond to high-magnification photos of the flake and flake thickness, respectively, from which the scaly morphology and size can be seen. Figure 2 The XRD diagram shown in c shows that there is metallic zinc and zinc oxide in the powder, but no zinc hydroxide phase. Figure 2 It can also be seen that the flaky powder D 50 It is about 5μm and less than 0.1μm thick. There is a certain amount of zinc oxide phase in the structure, and its thickness is estimated to be about 10 to 15nm.
[0050] (2) Dissolution
[0051] 5 g of curing agent solution, 60 g of solvent propylene glycol methyl ether and 1.2 g of dispersant were added into the container, and stirred at 20° C. for 0.5 hour. The speed of the stirrer was 40 rpm.
[0052] (3) Ball milling
[0053] The dissolved solution in step (2) was added into a ball mill, and 170 g of the flaky powder prepared in step (1) was added, and the mixture was ball milled for 4 hours.
[0054] (4) High-speed dispersion
[0055] The ball-milled slurry was poured into a high-speed disperser and dispersed at a line speed of about 100 m / s for 1 hour.
[0056] (5) Take 20g of epoxy resin solution, add 20g of water, stir at 20°C for 20 minutes and set aside. Add the dissolved epoxy resin solution to the slurry obtained in step (4) and stir evenly.
[0057] (6) After removing the loose rust on the surface of the rusted steel parts with an iron brush, add an appropriate amount of water according to the coating method. After obtaining the appropriate viscosity, paint the surface and let it dry.
[0058] According to the requirements of the neutral salt spray test performance test standard for paints and varnishes (GB / T1771-2007), the samples prepared by the present invention are tested in a neutral salt spray test machine for 4000 hours. Figure 3 As shown, there is no corrosion expansion at the scratched part of the sample surface, and no defects such as blistering, rust, and peeling at the non-scratched part. The salt spray time is higher than 600 hours in the zinc-rich primer standard (HG / T 3668-2009) and 2000 hours in the cold zinc coating standard (HG / T 4845-2015). Therefore, the waterborne epoxy heavy-duty anti-corrosion coating proposed in the present invention has more excellent performance.
[0059] Figure 4 Polarization curves of the waterborne epoxy heavy-duty anticorrosive coating prepared by the present invention and carbon steel in 5% NaCl solution. The results show that the corrosion potential of the waterborne epoxy heavy-duty anticorrosive coating prepared by the present invention is about 0.4 volts lower than that of bare steel.
[0060] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing a waterborne epoxy heavy-duty anticorrosive coating, characterized in that: Here are the steps: (1) Ball milling Add flaky powder, curing agent solution, dispersant and solvent in a weight ratio of 160-180:4.5-5.5:1-1.5:50-100 into a ball mill and grind for 4-6 hours, and no water is contained in the ball milling process; The flaky powder is a ZnO / Zn / ZnO three-layer structure flaky particle formed by in-situ forming a ZnO layer with a thickness of 0.1 to 20 nm on the surface of metal Zn. 50 In the range of 2 to 25 μm, the thickness is less than 0.1 μm; the preparation method of the flaky powder is: select D 50 Zn powder in the range of 5 to 50 μm is used as raw material and ball milled in a ball mill with a material: ball: water ratio of 1:1.5:0.8; the ball milling time is 1 to 4 hours, and the ball milled powder is kept at 250°C for 1 to 2 hours; (2) High-speed dispersion Pour the ball-milled slurry into a high-speed disperser and disperse it for 0.5 to 2 hours at a line speed greater than 50 m / s; (3) Slurry The dispersed slurry is poured out and placed in a container to form a gel-like thixotropic fluid, thus obtaining a filler-curing agent component; (4) Preparation of resin components Add epoxy resin and water into a container, and stir for 10 to 30 minutes at 5 to 35° C. to obtain a resin component; the epoxy resin in the resin component is added based on the weight ratio of the flaky powder in the dry coating being greater than 90%; (5) Preparation of coating The filler-curing agent component and the resin component are mixed evenly before coating, and the weight ratio of the flaky powder in the dry coating formed after coating on the substrate surface is greater than 90%. The flaky powder in the coating is alternately stacked in the form of layers to form the organizational structure of the anti-corrosion coating. The scales are conductive, and the coating forms a conductive whole.