Preparation method of tetraphenol fluorene and preparation method of tetraphenol fluorene-based epoxy resin

By preparing tetraphenolfluorene and tetraphenolfluorene-based epoxy resin under specific conditions, the problems of excessive phenol-ketone ratio and insufficient heat resistance of epoxy resin were solved, and an efficient, simple process and high performance were achieved. Tetraphenolfluorenyl epoxy resin.

CN116573989BActive Publication Date: 2024-10-01HUNAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310537503.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-10-01
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

In the preparation method of tetraphenolfluorene in the prior art, the phenol-ketone ratio is too large, making recovery difficult; the heat resistance and refractive index of the epoxy resin are insufficient, and the post-treatment process is complex, making separation and recovery difficult.

Method used

Under N2 sealing conditions, 2,7-dihydroxy-9-fluorenone, phenol and acid catalyst are reacted in a specific solvent. After water washing, distillation and recrystallization, tetraphenolfluorene is obtained; then tetraphenolfluorene and epoxy halogen are combined. Propane and protonated polar solvent are reacted under base catalysis, followed by filtration and recrystallization to prepare tetraphenol fluorenyl epoxy resin.

Benefits of technology

The raw material ratio of phenol and ketone is greatly reduced, and the yield and quality are improved. The prepared tetraphenolfluorene-based epoxy resin has low melt viscosity, high refractive index and good heat resistance, which can meet the requirements of high filler filling and no need for semiconductor packaging materials. Lead standard flux requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116573989B_ABST
    Figure CN116573989B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing tetraphenol fluorene and a method for preparing tetraphenol fluorene-based epoxy resin, wherein the method for preparing tetraphenol fluorene includes reacting 2,7-dihydroxy-9-fluorenone and phenol as raw materials in the presence of a solvent under N2 sealing conditions, and using an acid as a catalyst at a reflux temperature to obtain the obtained product. The method for preparing tetraphenol fluorene-based epoxy resin includes reacting tetraphenol fluorene and epihalohydrin as raw materials in the presence of a protonated polar solvent, using a base as a catalyst, and obtaining a crude product by post-treatment after the reaction is completed, and obtaining a tetraphenol fluorene-based epoxy resin by recrystallization. The method for preparing tetraphenol fluorene in the present invention can greatly reduce the raw material dosage ratio, and the yield is higher and the quality is better. The tetraphenol fluorene-based epoxy resin prepared by the present invention has the advantages of low melt viscosity, high refractive index, excellent heat resistance of resin cured product, etc., and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of organic synthesis, and in particular to a method for preparing tetraphenol fluorene and a method for preparing tetraphenol fluorene-based epoxy resin. Background Art

[0002] In semiconductor packaging, high filler filling is often used to reduce the water absorption and linear expansion coefficient of the sealant. Crystalline epoxy resin has the advantage of low melt viscosity in the molten state, which is conducive to the high filler filling of semiconductor packaging materials. With the advancement of the RoHS law and the development of human society, semiconductor packaging solder will continue to tend to be lead-free, and higher requirements are also put forward for the working temperature tolerance of the curing resin. For example, the aerospace field requires Tg>220℃, the floating of the lead eutectic standard flux in the welding of semiconductor packaging materials and flexible circuit substrates requires Tg≥260℃, and the floating Tg of lead-free standard flux is ≥288℃. In addition, the refractive index of the semiconductor chip and the transparent packaging material cannot be too different, otherwise it is easy to cause the external light extraction efficiency of the semiconductor chip to be too low. It is reported that the refractive indices of GaN and GaP, commonly used semiconductor chip materials, are 2.5 and 3.45 respectively, while the refractive indices of epoxy resins and silicone materials commonly used in semiconductor packaging are 1.450-1.550, and the refractive index needs to be improved.

[0003] Chinese patent document CN102659526A discloses a method for preparing a tetraphenol hydroxyfluorene compound, using dihydroxyfluorenone and substituted phenol as raw materials, using liquid acid as catalyst, preparing tetraphenol hydroxyfluorene by electrophilic substitution reaction of phenol ketone, washing with water-filtration to obtain a crude product, and then recrystallizing-filtration-drying to obtain fine tetraphenol hydroxyfluorene. In this method, the ratio of the amount of phenol ketone substance is too large, and the boiling point of phenol is high, which has the problem of difficult recovery. In addition, the crude product exists in a solid state during the water washing and acid removal process of this method, which will produce a large amount of water-acid-phenol mixture.

[0004] Japanese patent document JP4915896B2 discloses a method for preparing a high melting point crystalline epoxy resin, wherein the method uses bisphenol fluorene and epihalohydrin as raw materials, with or without alcohol and aprotic polar solvent conditions, with solid or liquid alkali metal hydroxide as catalyst, with or without quaternary ammonium salt phase transfer catalyst, adopts open-loop-closed loop batch alkali addition method to prepare epoxy resin, and then adopts water washing-concentration-crystallization precipitation method to prepare crystalline bisphenol fluorene epoxy resin (DGEBF). However, the method adopts water washing-concentration-crystallization precipitation method, that is, during post-treatment, part of epichlorohydrin is first distilled out, and then a mixture of a poor solvent and water is added, and a method for separating product crystals while removing epichlorohydrin by azeotropic co-extraction is adopted. In this method, a ternary mixture of water-methanol-epichlorohydrin is generated during concentration, and there is a problem of difficulty in separation and recovery.

[0005] Chinese patent document CN111574482A discloses a method for the efficient catalytic synthesis of epoxy bisphenol fluorene, which adopts a two-step method to prepare bisphenol fluorene epoxy resin, with bisphenol fluorene and epichlorohydrin as raw materials, in the presence of a phase transfer catalyst, with an organic base or an inorganic base as a catalyst, through an open-loop-closed loop process, after completion, a crude product is obtained by washing and desolvation process, and then a polar solvent is used for recrystallization to obtain crystalline epoxy bisphenol fluorene (DGEBF). The raw material used in this method is bisphenol fluorene, and the heat resistance of the obtained epoxy resin is not good enough, and the method adopts a phase transfer catalyst method to prepare the product, and recovery and wastewater post-treatment are difficult.

[0006] The literature published by Liu et al. (Liu W, Qiu Q, Wang J, et al. Preparation and properties of one epoxy system bearing fluorene moieties [J]. Journal of applied polymer science, 2009, 113 (2): 1289-1297) uses bisphenol fluorene and epihalohydrin as raw materials, dioxane as solvent, 50% NaOH as catalyst in the presence of a phase transfer catalyst, and adopts an open-loop-closed-loop batch alkali method to prepare epoxy resin, then uses a method of water washing and desalting-water precipitation-filtration to obtain a crude product, and then recrystallizes to obtain a crystalline bisphenol fluorene epoxy resin (DGEBF). The cured product DGEBF / DDM obtained by curing with the curing agent 4,4-diaminodiphenylmethane (DDM) has a glass transition temperature of 248.0°C. The post-treatment method adopted in this method is to obtain a crude product by water washing and desalting-water precipitation-filtration, that is, after post-treatment and desalting, water, a poor solvent for the resin, is directly added to the mixed solution to precipitate, and the crude product is filtered and then recrystallized to obtain a crystalline product. When water is added for precipitation, a ternary mixture of water, dioxane and epichlorohydrin is formed, which is difficult to separate and recover. Summary of the invention

[0007] The technical problem to be solved by the present invention is to overcome the shortcomings of the prior art and provide a method for preparing tetraphenolfluorene which can significantly reduce the raw material usage ratio, has higher yield and better quality, and also provides a method for preparing tetraphenolfluorene-based epoxy resin with low melt viscosity, high refractive index and good heat resistance of resin cured product.

[0008] In order to solve the above technical problems, the present invention adopts the following technical solutions.

[0009] A method for preparing tetraphenol fluorene comprises the following steps:

[0010] Under N2 sealing conditions, 2,7-dihydroxy-9-fluorenone, phenol, solvent and acid catalyst are added into a reaction container, heated and stirred evenly, and the reaction is maintained at reflux temperature for 3h to 24h, and then washed with water, the solvent and excess phenol are removed by distillation, and vacuum dried to obtain a crude tetraphenol fluorene, and tetraphenol fluorene is obtained after recrystallization; wherein the molar ratio of the phenol to the 2,7-dihydroxy-9-fluorenone is 4 to 8:1, and the solvent is one or more of ethyl acetate, toluene and nitrobenzene.

[0011] In the above-mentioned method for preparing tetraphenolfluorene, preferably, the mass of the solvent is 20wt% to 300wt% of the mass of 2,7-dihydroxy-9-fluorenone, the mass of the acid catalyst is 20wt% to 100wt% of the mass of 2,7-dihydroxy-9-fluorenone, and the reaction time is 5h to 24h; the acid catalyst is an inorganic acid or an organic acid, the inorganic acid includes hydrochloric acid or sulfuric acid, the organic acid includes one or more of p-toluenesulfonic acid, methanesulfonic acid, mercaptoethanesulfonic acid, mercaptopropanesulfonic acid and mercaptocarboxylic acid, and the mercaptocarboxylic acid includes thioacetic acid and / or mercaptopropionic acid.

[0012] In the above-mentioned method for preparing tetraphenol fluorene, preferably, the molar ratio of the phenol to 2,7-dihydroxy-9-fluorenone is 5 to 7:1, the mass of the solvent is 20wt% to 100wt% of the mass of 2,7-dihydroxy-9-fluorenone, and the mass of the acid catalyst is 30wt% to 60wt% of the mass of 2,7-dihydroxy-9-fluorenone.

[0013] As a general technical concept, the present invention also provides a method for preparing a tetraphenol fluorene-based epoxy resin, comprising the following steps:

[0014] S1. Add tetraphenol fluorene, epihalohydrin and protonated polar solvent into a reaction vessel, heat to reflux temperature, stir and mix evenly, add base catalyst in batches within 1.5h to 2h, and maintain reflux temperature for reaction for 2h to 6h. After the reaction is completed, filter, wash with water, and recover the solvent and excess raw materials by vacuum distillation to obtain a crude tetraphenol fluorene epoxy resin;

[0015] S2. Recrystallize the crude tetraphenol fluorene-based epoxy resin obtained above to obtain tetraphenol fluorene-based epoxy resin.

[0016] In the above-mentioned method for preparing tetraphenol fluorene-based epoxy resin, preferably, in step S1, the tetraphenol fluorene is tetraphenol fluorene prepared by the above-mentioned method for preparing tetraphenol fluorene.

[0017] In the above-mentioned method for preparing tetraphenol fluorene-based epoxy resin, preferably, in step S1, the molar ratio of the epihalohydrin to tetraphenol fluorene is 8 to 60:1, and the mass of the protonated polar solvent is 30 wt% to 400 wt% of the mass of tetraphenol fluorene.

[0018] In the above-mentioned method for preparing tetraphenolfluorene-based epoxy resin, preferably, in step S1, the epihalohydrin includes one or both of epichlorohydrin and epibromohydrin.

[0019] In the above-mentioned method for preparing tetraphenolfluorene-based epoxy resin, preferably, in step S1, the protonated polar solvent includes one or more of methanol, ethanol, isopropanol, n-butanol, diethylene glycol dimethyl ether, ethylene glycol monobutyl ether, ethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol monoethyl ether, dipropylene glycol monobutyl ether and dipropylene glycol monoethyl ether.

[0020] In the above-mentioned method for preparing tetraphenolfluorene-based epoxy resin, preferably, in step S1, the base catalyst is an alkali metal hydroxide solid or an alkali metal hydroxide solution, the alkali metal hydroxide includes sodium hydroxide or potassium hydroxide, the molar ratio of the alkali metal hydroxide to tetraphenolfluorene is 2 to 6:1, and the concentration of the alkali metal hydroxide solution is 30wt% to 50wt%; when the base catalyst is an alkali metal hydroxide solution, reflux dehydration is required under vacuum conditions.

[0021] In the above-mentioned method for preparing tetraphenol fluorene-based epoxy resin, preferably, in step S1, the molar ratio of the epihalohydrin to tetraphenol fluorene is 12 to 48:1; the molar ratio of the alkali metal hydroxide to tetraphenol fluorene is 3 to 5:1, and the mass of the protonated polar solvent is 40wt% to 200wt% of the mass of tetraphenol fluorene.

[0022] In the above-mentioned method for preparing tetraphenolfluorene-based epoxy resin, preferably, in step S2, the solvent used for the recrystallization includes one or more of acetone, acetonitrile, dioxane, isopropanol, ethanol, methanol and dichloromethane.

[0023] In the present invention, the reaction equation of tetraphenol fluorene is as shown in the following formula (1). The full name of tetraphenol fluorene is 2,7-dihydroxy 9,9'-bis(4-hydroxyphenyl)fluorene.

[0024]

[0025] In the present invention, the synthesis reaction equation of tetraphenolfluorene-based epoxy resin is shown in the following formula (2).

[0026]

[0027] Compared with the prior art, the advantages of the present invention are:

[0028] 1. The present invention provides a method for preparing tetraphenol fluorene. The applicant has found that when the method uses one or more of the specific solvents ethyl acetate, toluene and nitrobenzene, the phenol-ketone ratio can be greatly reduced. The technical solution of the patent document CN102659526A in the background technology is an existing typical method for preparing tetraphenol fluorene, which has a phenol-ketone ratio of 8-16:1, a high amount of phenol, easy oxidation at high temperature, and difficult recycling. The present invention uses a solvent to carry out the reaction, which can greatly reduce the phenol-ketone raw material dosage ratio. At the same time, the tetraphenol fluorene prepared by the present invention has a higher yield and better quality. In addition, the post-treatment process of the present invention is also significantly better than the prior art. The prior art uses water washing-suction filtration to obtain a crude tetraphenol hydroxyfluorene product, and the product exists in a solid state, which will produce a large amount of water-acid-phenol mixture. However, since the present invention has a solvent involved in the reaction, the reactant exists in a solution state, and the operation process of washing and removing acid to obtain a crude product is simpler, the washing is more sufficient, and less wastewater is generated.

[0029] 2. The present invention also provides a method for preparing a tetraphenol fluorene-based epoxy resin. The prepared tetraphenol fluorene-based epoxy resin has low melt viscosity, high refractive index (1.61), and good heat resistance of the cured resin (T g The low melt viscosity is conducive to high filler filling of sealing materials, the high refractive index is conducive to improving the luminous efficiency of semiconductor packaging materials, and the resin cured product has good heat resistance and can meet the requirements of semiconductor packaging lead-free standard flux floating Tg ≥ 288 ° C. The preparation method of the present invention can obtain the product by a one-step method, has the characteristics of short process, simple operation, good repeatability, easier recovery of excess epihalohydrin and more energy saving, and has good application prospects in the field of high-performance epoxy resins for semiconductor packaging.

[0030] Compared with Japanese patent document JP4915896B2 in the background technology, the present invention uses different raw materials, the resin cured product of the present invention has better heat resistance, and the post-treatment method of the present invention is better. The above patent document adopts a water washing-concentration-crystallization precipitation method, that is, during post-treatment, a part of epichlorohydrin is first evaporated, and then a mixture of a poor solvent and water is added, and a method of azeotropic removal of epichlorohydrin is adopted while precipitating product crystals. In this method, a ternary mixture of water-methanol-epichlorohydrin is generated during concentration, and there is a problem of difficulty in separation and recovery. However, during post-treatment, the present invention adopts the method of completely evaporating the epichlorohydrin, and then recrystallizing and drying to obtain the product. In the present invention, the epichlorohydrin is evaporated once, and recovery is easier and more energy-saving.

[0031] Compared with the Chinese patent document CN111574482A in the background technology, the present invention uses different raw materials, and the resin cured product of the present invention has better heat resistance. In addition, the above patent document adopts a phase transfer catalyst method to prepare the product, which is difficult to recycle and post-process wastewater. The present invention adopts a one-step method to prepare a crude epoxy resin, and then adopts a recrystallization method to prepare a tetraphenol fluorene-based epoxy resin.

[0032] Compared with the technical scheme in the document published by Liu et al. in the background technology, the present invention uses different raw materials. The raw material used in the document is bisphenol fluorene, and the raw material used in the curing of the present invention is tetraphenol fluorene. The resin cured product obtained by the present invention has better heat resistance. The document adopts a phase transfer catalyst method to prepare the product, and the present invention adopts a one-step method to prepare a crude epoxy resin, and then adopts a recrystallization method to prepare a tetraphenol fluorene-based epoxy resin. The present invention is different from the post-treatment method adopted in the document. The document adopts a water washing desalination-water precipitation-suction filtration method to obtain a crude product, that is, after post-treatment desalination, a poor solvent of the resin is directly added to the mixed solution to precipitate, and the crude product is obtained by suction filtration and then recrystallization to obtain a crystalline product. When adding water to precipitate, a ternary mixture of water, dioxane, and epichlorohydrin will be formed, and there is a problem of difficulty in separation and recovery. The present invention takes all the epihalohydrin to be steamed out during post-treatment, and then recrystallized and dried to obtain the product. Compared with the post-treatment in the document, all the epihalohydrin is directly steamed out, and recovery is easier and more energy-saving. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of tetraphenolfluorene in Example 1 of the present invention.

[0034] Figure 2 This is the mass spectrum of tetraphenolfluorene in Example 1 of the present invention.

[0035] Figure 3 This is an infrared spectrum test chart of the tetraphenolfluorene-based epoxy resin in Example 2 of the present invention.

[0036] Figure 4 This is the hydrogen nuclear magnetic resonance spectrum of the tetraphenolfluorene-based epoxy resin in Example 2 of the present invention.

[0037] Figure 5 This is the mass spectrum of the tetraphenolfluorene-based epoxy resin in Example 2 of the present invention.

[0038] Figure 6 This is the DMA diagram of the DDM cured product in Example 2 of the present invention.

[0039] Figure 7 This is the TG diagram of the DDM cured product in Example 2 of the present invention. DETAILED DESCRIPTION

[0040] The present invention is further described below in conjunction with the accompanying drawings and specific preferred embodiments, but the protection scope of the present invention is not limited thereby. The materials and instruments used in the following embodiments are all commercially available.

[0041] Example 1

[0042] A method for preparing tetraphenol fluorene of the present invention comprises the following steps:

[0043] Under nitrogen sealing conditions, 63.6 g of 2,7-dihydroxy-9-fluorenone (0.3 mol), 169.6 g of phenol (1.8 mol), 65 mL of ethyl acetate, 15 mL of 98 wt% concentrated sulfuric acid and 6 mL of mercaptopropionic acid were added in sequence into a three-necked flask equipped with a stirrer, a reflux condenser and a temperature sensor, heated to reflux temperature and stirred evenly, and the reflux temperature was maintained at 60°C for 9 hours. After the reaction was completed, the mixture was washed with water to neutrality, the solvent and excess phenol were recovered by vacuum distillation, and the crude product was obtained. Recrystallization gave 96.0 g of tetraphenolfluorene product with a yield of 83.8% and a melting point of 325-326°C.

[0044] The H NMR spectrum of this product is Figure 1 As shown, 1 H NMR (400MHz, DMSO-d6, ppm), δ9.29 (5, 2H), 9.28 (1, 2H), 7.47 (7, 2H), 6.83 (3, 4H), 6.70-6.67 (6, 2H), 6.64 (4, 2H), 6.62 (2, 4H). The mass spectrometry test results are as follows Figure 2 As shown, the theoretical molecular weight of tetraphenol fluorene is 382.12, and the molecular weight obtained by testing is close to the theoretical value. The above results show that the product is indeed tetraphenol fluorene.

[0045] Comparative Example 1

[0046] A method for preparing tetraphenol fluorene is basically the same as the preparation process of Example 1, except that the solvent ethyl acetate in Example 1 is replaced by tetrahydrofuran. The method obtains 7.3 g of tetraphenol fluorene product with a yield of 6.4% and a melting point of 325-326°C.

[0047] Comparative Example 2

[0048] A method for preparing tetraphenol fluorene is basically the same as the preparation process of Example 1, except that the solvent ethyl acetate in Example 1 is replaced by ethanol. After the reaction is completed, the mixture is washed with water until neutral, and the solvent and phenol are recovered by vacuum distillation to obtain reddish brown particles. Chromatographic analysis shows that the particles are mainly 2,7-dihydroxy-9-fluorenone, and almost no product is generated.

[0049] Example 2

[0050] A method for preparing a tetraphenol fluorene-based epoxy resin of the present invention comprises the following steps:

[0051] S1, 96.0g tetraphenol fluorene (about 0.25mol), 400mL epichlorohydrin (5mol), and 150mL ethanol prepared in Example 1 were placed in a four-mouth round-bottom flask equipped with a reflux condenser and agitator, heated to a reflux temperature of 80°C, stirred and mixed evenly, tetraphenol fluorene was completely dissolved, and then 40.0g solid NaOH was added in batches within 2h, and the reflux temperature was maintained for 2h after the addition was completed. After the reaction was completed, the filtrate was filtered, and the filtrate was washed with hot water greater than 70°C until neutral, and then the solvent and unreacted epichlorohydrin were recovered by reduced pressure distillation to obtain a crude tetraphenol fluorene-based epoxy resin.

[0052] S2. The crude product was recrystallized and dried using a V / V 1:2 acetone-methanol composite solvent to obtain 129.2 g of the target product tetraphenolfluorene-based epoxy resin with a yield of 85.3%, an epoxy equivalent of 169 g / eq, and a refractive index of 1.61.

[0053] The infrared spectrum test results of the target product are shown in Figure 3 , 914cm -1 The characteristic peak of epoxy group appeared at 3275cm -1 The characteristic peak of the hydroxyl group at the position disappears. Figure 4 The attribution of the characteristic peaks is shown in Table 1. Each peak can be attributed to the hydrogen at the corresponding chemical shift. Figure 5 , where M represents the molecular weight of the product tetraphenol fluorene epoxy resin. The theoretical molecular weight of tetraphenol fluorene epoxy resin when the degree of polymerization n=0 is 606.49, which is consistent with the results. + represents 1 fluorenyl tetraglycidyl ether and 1 Na + The price is the same, and the rest is the same.

[0054] The target product was used as raw material to prepare DDM cured product. The DMA and TG test graphs of the cured product are shown in Figure 6 and Figure 7 , glass transition temperature (T g ) reached 298.81℃, the temperature of 5% weight loss (T 5% ) is 358.12℃.

[0055] Table 1 Target products of Example 1 1 H NMR results table

[0056] Hydrogen position δ(measured value) δ(simulated value) 11 7.72 7.90 4,5,6,10 7.03-6.75 7.18-6.85 7 4.26 4.17 3 3.85-3.68 3.92 2,8 3.28 3.04 1,9 2.73-2.59 2.61-2.36

[0057] Example 3

[0058] A method for preparing a tetraphenol fluorene-based epoxy resin of the present invention comprises the following steps:

[0059] S1, 96.0g tetraphenol fluorene (about 0.25mol), 400mL epichlorohydrin (5mol), and 150mL ethanol prepared in Example 1 were placed in a four-mouth round-bottom flask equipped with a reflux condenser and a stirrer, heated to a reflux temperature of 80°C, stirred and mixed evenly, and the tetraphenol fluorene was completely dissolved, and then 100.0g of 40wt% NaOH solution was added in batches within 2h and a vacuum reflux water separation environment was maintained. After the addition was completed, the reflux temperature was maintained for 2h. After the reaction was completed, it was cooled and filtered, and the filtrate was washed with hot water until neutral, and then the solvent and unreacted epichlorohydrin were recovered by reduced pressure distillation to obtain a crude tetraphenol fluorene-based epoxy resin.

[0060] S2. The crude product was recrystallized using a V / V 1:2 acetone-methanol composite solvent. The crystals were filtered and dried to obtain 132.0 g of the target product, tetraphenolfluorene-based epoxy resin, with a yield of 87.1%, an epoxy equivalent of 167 g / eq, and a refractive index of 1.61.

[0061] Example 4

[0062] A method for preparing a tetraphenol fluorene-based epoxy resin of the present invention comprises the following steps:

[0063] S1. Put 96.0g tetraphenol fluorene (about 0.25mol), 400mL epichlorohydrin (5mol) and 150mL ethylene glycol monoethyl ether prepared in Example 1 into a four-mouth round-bottom flask equipped with a reflux condenser and a stirrer, heat to a reflux temperature of 80°C, stir and mix evenly, and the tetraphenol fluorene is completely dissolved. Then, 40.0g solid NaOH is added in batches within 2h. After the addition is completed, the reflux temperature is maintained for 2h. Then filter, wash the filtrate with hot water greater than 70°C until neutral, and then distill under reduced pressure to recover the solvent and unreacted epichlorohydrin to obtain a crude product.

[0064] S2. The crude product was recrystallized and dried using an acetone-methanol composite solvent with a V / V ratio of 1:2 to obtain 121.4 g of the target product, tetraphenolfluorene-based epoxy resin, with a yield of 80.4%, an epoxy equivalent of 174 g / eq, and a refractive index of 1.61.

[0065] Comparative Example 3

[0066] A method for preparing a tetraphenol fluorene-based epoxy resin, the preparation process is basically the same as that of Example 2, except that in step S1, 150 mL of dimethyl sulfoxide is used as a solvent. The target product tetraphenol fluorene-based epoxy resin is 108.1 g, with a yield of 71.7% and an epoxy equivalent of 194 g / eq.

[0067] Comparative Example 4

[0068] A method for preparing a tetraphenol fluorene-based epoxy resin, the preparation process is basically the same as that of Example 2, except that in step S1, 150 mL of dioxane is used as a solvent. The target product tetraphenol fluorene-based epoxy resin is 114.5 g, with a yield of 75.8% and an epoxy equivalent of 184 g / eq.

[0069] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as above in the preferred embodiment, it is not used to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent replacement, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention, still fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for preparing tetraphenol fluorene, characterized in that: The following steps are involved: Under N2 sealing conditions, 2,7-dihydroxy-9-fluorenone, phenol, solvent and acid catalyst are added into a reaction container, heated and stirred evenly, and the reaction is maintained at reflux temperature for 3h to 24h, and then washed with water, the solvent and excess phenol are removed by distillation, and vacuum dried to obtain a crude tetraphenol fluorene, and tetraphenol fluorene is obtained after recrystallization; wherein the molar ratio of the phenol to the 2,7-dihydroxy-9-fluorenone is 4 to 8:1, and the solvent is ethyl acetate.

2. The method for preparing tetraphenol fluorene according to claim 1, characterized in that: The mass of the solvent is 20wt% to 300wt% of the mass of 2,7-dihydroxy-9-fluorenone, the mass of the acid catalyst is 20wt% to 100wt% of the mass of 2,7-dihydroxy-9-fluorenone, and the reaction time is 5h to 24h; the acid catalyst is an inorganic acid or an organic acid, the inorganic acid includes hydrochloric acid or sulfuric acid, the organic acid includes one or more of p-toluenesulfonic acid, methanesulfonic acid, mercaptoethanesulfonic acid, mercaptopropanesulfonic acid and mercaptocarboxylic acid, and the mercaptocarboxylic acid includes mercaptoacetic acid and / or mercaptopropionic acid.

3. The method for preparing tetraphenol fluorene according to claim 2, characterized in that: The molar ratio of the phenol to the 2,7-dihydroxy-9-fluorenone is 5-7:1, the mass of the solvent is 20wt%-100wt% of the mass of the 2,7-dihydroxy-9-fluorenone, and the mass of the acid catalyst is 30wt%-60wt% of the mass of the 2,7-dihydroxy-9-fluorenone.

4. A method for preparing a tetraphenol fluorene-based epoxy resin, characterized in that: The following steps are involved: S1. Add tetraphenolfluorene, epihalohydrin and protonated polar solvent into a reaction vessel, heat to reflux temperature, stir and mix evenly, add base catalyst in batches within 1.5h to 2h, maintain reflux temperature and react for 2h to 6h, filter, wash with water, and distill under reduced pressure to recover solvent and excess raw materials after the reaction is completed to obtain a crude tetraphenolfluorene epoxy resin; the protonated polar solvent is one or more of methanol, ethanol, isopropanol, n-butanol, ethylene glycol monobutyl ether, ethylene glycol monoethyl ether, diethylene glycol monobutyl ether, diethylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol monoethyl ether, dipropylene glycol monobutyl ether and dipropylene glycol monoethyl ether; The preparation method of the tetraphenol fluorene is as follows: Under N2 sealing conditions, 2,7-dihydroxy-9-fluorenone, phenol, solvent and acid catalyst are added to a reaction container, heated and stirred evenly, and reacted at reflux temperature for 3h to 24h, then washed with water, distilled to remove the solvent and excess phenol, and vacuum dried to obtain a crude tetraphenol fluorene, and after recrystallization, tetraphenol fluorene is obtained; wherein the molar ratio of the phenol to the 2,7-dihydroxy-9-fluorenone is 4 to 8:1, and the solvent is ethyl acetate; S2. Recrystallize the crude tetraphenol fluorene-based epoxy resin obtained above to obtain tetraphenol fluorene-based epoxy resin.

5. The method for preparing a tetraphenol fluorene-based epoxy resin according to claim 4, characterized in that: In step S1, the molar ratio of the epihalohydrin to tetraphenol fluorene is 8 to 60:1, and the mass of the protonated polar solvent is 30 wt% to 400 wt% of the mass of tetraphenol fluorene.

6. The method for preparing a tetraphenol fluorene-based epoxy resin according to claim 5, characterized in that: In step S1, the epihalohydrin includes one or both of epichlorohydrin and epibromohydrin; The base catalyst is an alkali metal hydroxide solid or an alkali metal hydroxide solution, the alkali metal hydroxide includes sodium hydroxide or potassium hydroxide, the amount ratio of the alkali metal hydroxide to tetraphenolfluorene is 2 to 6:1, and the concentration of the alkali metal hydroxide solution is 30 wt% to 50 wt%; when the base catalyst is an alkali metal hydroxide solution, reflux dehydration is required under vacuum conditions.

7. The method for preparing a tetraphenol fluorene-based epoxy resin according to claim 6, characterized in that: In step S1, the molar ratio of the epihalohydrin to tetraphenol fluorene is 12-48:1; the molar ratio of the alkali metal hydroxide to tetraphenol fluorene is 3-5:1, and the mass of the protonated polar solvent is 40wt%-200wt% of the mass of tetraphenol fluorene.

8. The method for preparing a tetraphenol fluorene-based epoxy resin according to any one of claims 4 to 7, characterized in that: In step S2, the solvent used for the recrystallization includes one or more of acetone, acetonitrile, dioxane, isopropanol, ethanol, methanol and dichloromethane.