A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating and preparation method thereof
By introducing two-dimensional nanomaterials and phenoamines into solvent-free epoxy coatings, high-efficiency curing agents and enhanced shielding components are formed, the problem of insufficient wear resistance and corrosion resistance of the coating is solved, and excellent shielding protection performance is achieved and long-term wear resistance.
Patent Information
- Application Number
- CN202310451701.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-25
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-04-25
AI Technical Summary
Existing solvent-free epoxy coatings have poor performance in wear resistance, shielding and corrosion resistance, mainly due to insufficient hardness caused by total reliance on crosslinking reactions and lack of effective curing agent neutralization reactions and shielding materials.
Using two-dimensional nanomaterials (such as two-dimensional carbon nanotubes and two-dimensional nanographene) combined with epoxy resin and phenoamine, the curing agent formed by neutralization reaction and secondary neutralization reaction is combined with glass powder to improve the coating. The wear resistance and corrosion resistance of the product are enhanced by carbon nanotubes and two-dimensional nanographene.
The excellent corrosion resistance, wear resistance and enhanced shielding protection performance of the paint are achieved. The paint film remains intact for more than 8000 hours in neutral salt spray test, significantly improving corrosion resistance.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and specifically relates to a two-dimensional nano-modified solvent-free epoxy internal drag reduction coating and a preparation method thereof. Background Art
[0002] At present, the existing solvent-free epoxy coating mainly adopts the solvent-free epoxy coating made by the reaction of high molecular weight epoxy and alicyclic amine modified polyamide. For example, high molecular weight epoxy resin, epoxy functional group active diluent, polyamide wax, titanium dioxide are used as paint components, and alicyclic amine modified polyamide is used as curing agent component. However, since it completely relies on the hardness of the paint film generated by cross-linking reaction to solve the problem of wear resistance, it causes poor wear resistance; since it completely relies on pigments and fillers and the burden of epoxy resin itself to solve the problem of coating shielding, its shielding property is also poor; at the same time, the paint film formed directly by the reaction of alicyclic amine modified polyamide and epoxy, the curing agent part does not undergo secondary neutralization reaction, so it has poor corrosion resistance and low drag reduction.
[0003] Therefore, it is of great significance to develop a solvent-free epoxy internal drag reduction coating with excellent corrosion resistance, wear resistance and drag reduction properties. Summary of the invention
[0004] The invention provides a two-dimensional nano-modified solvent-free epoxy internal drag-reducing coating and a preparation method thereof. The coating has good corrosion resistance, wear resistance and drag-reducing properties and also has good shielding protection performance.
[0005] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which is composed of 85-90% of a paint component and 10-15% of a curing agent component, based on a weight ratio of 100%;
[0006] The paint component is composed of the following raw materials at a weight ratio of 100%:
[0007] Epoxy functional group active diluent 0.2-1%, hydrogenated castor oil 2-4%, polyamide wax 0.2-1%, pigment 8-35%, two-dimensional carbon nanotube 2-6%, two-dimensional nanographene 2-4%, fluorine-modified polyacrylate copolymer 0.1-1%, glass powder 1-5%, and the balance is epoxy resin.
[0008] Preferably, the curing agent component is composed of the following raw materials based on a weight ratio of 100%: 3-8% benzyl alcohol, 2-10% salicylic acid, 10-30% phenalkamine, 5-20% epoxy resin, and the balance is phenolic modified polyamide.
[0009] Preferably, the epoxy functional group reactive diluent is glycidol.
[0010] Preferably, the pigment is red iron oxide.
[0011] Preferably, the paint component is composed of the following raw materials: 0.2-1% epoxy functional group active diluent, 2-4% hydrogenated castor oil, 0.2-1% polyamide wax, 8-25% pigment, 3-5% two-dimensional carbon nanotubes, 2-3.8% two-dimensional nanographene, 0.1-1% fluorine-modified polyacrylate copolymer, 1-5% glass powder, and the balance is epoxy resin;
[0012] The curing agent component is composed of the following raw materials: 3-7.8% benzyl alcohol, 2-10% salicylic acid, 10-28% phenalkamine, 8-17% epoxy resin, and the balance is phenolic modified polyamide.
[0013] Preferably, the paint component is composed of the following raw materials: 0.2-0.5% epoxy functional group active diluent, 2-3% hydrogenated castor oil, 0.5-1% polyamide wax, 10-15% pigment, 3-4% two-dimensional carbon nanotubes, 2.2-3% two-dimensional nanographene, 0.1-1% fluorine-modified polyacrylate copolymer, 2-4% glass powder, and the balance is epoxy resin;
[0014] The curing agent component is composed of the following raw materials: 6-7% benzyl alcohol, 8-10% salicylic acid, 20-25% phenalkamine, 8-12% epoxy resin, and the balance is phenolic modified polyamide.
[0015] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reduction coating comprises the following steps:
[0016] (1) Preparing a paint component: mixing epoxy resin, epoxy functional group active diluent, hydrogenated castor oil, and polyamide wax, stirring until uniformly dispersed, and then sequentially adding pigment, two-dimensional carbon nanotubes, two-dimensional nanographene, fluorine-modified polyacrylate copolymer, and glass powder thereto, stirring until uniformly dispersed, to obtain a paint component;
[0017] (2) preparing a curing agent component: mixing benzyl alcohol, salicylic acid, phenolic amine and epoxy resin under stirring, keeping the mixture at 90-100° C. for 3-5 hours, then adding phenolic modified polyamide thereto, stirring for 5-10 minutes, and obtaining a curing agent component;
[0018] (3) Preparing coating: mixing the paint component and the curing agent component according to a certain proportion.
[0019] Advantages of the present invention:
[0020] (1) The coating provided by the present invention uses epoxy resin as a carrier, and firstly neutralizes phenolic amine with epoxy to prepare a curing agent component, and then performs a curing reaction with the epoxy in the paint part, and has excellent corrosion resistance, wear resistance, and drag reduction properties;
[0021] (2) The ingenious combination of carbon nanotubes and two-dimensional nanographene materials as long-term shielding protection increases the anti-shielding performance of the coating;
[0022] (3) Increase long-term and lasting wear resistance by adding glass powder; use polyamide, epoxy resin, and phenolic amine to perform a secondary neutralization reaction under the action of salicylic acid as an overall reaction cross-linking curing agent, and after the secondary neutralization reaction, comprehensively improve the wear resistance and anti-corrosion performance of the coating;
[0023] (4) The paint film is intact and has good corrosion resistance after being tested for more than 8000 hours in neutral salt spray test. DETAILED DESCRIPTION
[0024] In the embodiment of the present invention, the model of the phenolic modified polyamide is BASF EC201, and the model of the fluorine modified polyacrylate copolymer is Deqian 839.
[0025] Example 1
[0026] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which, by weight ratio of 100%, consists of 85% of a paint component and 15% of a curing agent component;
[0027] The paint component is composed of the following raw materials according to a weight ratio of 100%: 49% epoxy resin, 1% glycidol, 4% hydrogenated castor oil, 1% polyamide wax, 35% red iron oxide, 4% two-dimensional carbon nanotubes, 4% two-dimensional nanographene, 1% fluorine-modified polyacrylate copolymer, and 1% glass powder;
[0028] The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 8% benzyl alcohol, 10% salicylic acid, 30% phenalkamine, 20% epoxy resin, and 32% phenolic modified polyamide.
[0029] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reduction coating comprises the following steps:
[0030] (1) Preparing a paint component: mixing epoxy resin, epoxy functional group active diluent glycidol, hydrogenated castor oil, and polyamide wax, stirring at high speed for 0.2 h to disperse uniformly, then adding pigment red iron oxide, two-dimensional carbon nanotubes, two-dimensional nanographene, fluorine-modified polyacrylate copolymer, and glass powder in sequence, stirring until dispersed uniformly, to obtain a paint component;
[0031] (2) preparing a curing agent component: mixing benzyl alcohol, salicylic acid, phenolic amine and epoxy resin under stirring, keeping the mixture at 90° C. for 5 h, then adding phenolic modified polyamide thereto, stirring for 5 min, and obtaining a curing agent component;
[0032] (3) Preparing coating: mixing the paint component and the curing agent component according to a certain proportion.
[0033] Example 2
[0034] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which, by weight ratio of 100%, consists of 85% of a paint component and 15% of a curing agent component;
[0035] The paint component is composed of the following raw materials according to a weight ratio of 100%: 47.5% epoxy resin, 0.2% glycidol, 2% hydrogenated castor oil, 0.2% polyamide wax, 35% red iron oxide, 6% two-dimensional carbon nanotubes, 4% two-dimensional nanographene, 0.1% fluorine-modified polyacrylate copolymer, and 5% glass powder;
[0036] The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 8% benzyl alcohol, 2% salicylic acid, 10% phenalkamine, 20% epoxy resin, and 60% phenolic modified polyamide.
[0037] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reducing coating is the same as that of Example 1.
[0038] Example 3
[0039] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which, by weight ratio of 100%, consists of 85% of a paint component and 15% of a curing agent component;
[0040] The paint component is composed of the following raw materials according to a weight ratio of 100%: 79% epoxy resin, 0.5% glycidol, 2% hydrogenated castor oil, 0.5% polyamide wax, 8% red iron oxide, 2% two-dimensional carbon nanotubes, 2% two-dimensional nanographene, 1% fluorine-modified polyacrylate copolymer, and 5% glass powder;
[0041] The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 3% benzyl alcohol, 10% salicylic acid, 30% phenalkamine, 5% epoxy resin, and 52% phenolic modified polyamide.
[0042] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reducing coating is the same as that of Example 1.
[0043] Example 4
[0044] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which, by weight ratio of 100%, consists of 90% of a paint component and 10% of a curing agent component;
[0045] The paint component is composed of the following raw materials according to a weight ratio of 100%: 66% epoxy resin, 0.2% glycidol, 2% hydrogenated castor oil, 0.7% polyamide wax, 25% red iron oxide, 3% two-dimensional carbon nanotubes, 2% two-dimensional nanographene, 0.1% fluorine-modified polyacrylate copolymer, and 1% glass powder;
[0046] The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 3% benzyl alcohol, 2% salicylic acid, 28% phenalkamine, 17% epoxy resin, and 50% phenolic modified polyamide.
[0047] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reduction coating comprises the following steps:
[0048] (1) Preparing a paint component: mixing epoxy resin, epoxy functional group active diluent glycidol, hydrogenated castor oil, and polyamide wax, stirring at high speed for 0.3 h to disperse uniformly, then adding pigment red iron oxide, two-dimensional carbon nanotubes, two-dimensional nanographene, fluorine-modified polyacrylate copolymer, and glass powder in sequence, stirring until dispersed uniformly, to obtain a paint component;
[0049] (2) preparing a curing agent component: mixing benzyl alcohol, salicylic acid, phenolic amine and epoxy resin under stirring, keeping the mixture at 100° C. for 3 h, then adding phenolic modified polyamide thereto, stirring for 10 min, and obtaining a curing agent component;
[0050] (3) Preparing coating: mixing the paint component and the curing agent component according to a certain proportion.
[0051] Example 5
[0052] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which, by weight ratio of 100%, consists of 90% of a paint component and 10% of a curing agent component;
[0053] The paint component is composed of the following raw materials according to a weight ratio of 100%: 76.2% epoxy resin, 1% glycidol, 2% hydrogenated castor oil, 1% polyamide wax, 8% red iron oxide, 5% two-dimensional carbon nanotubes, 3.8% two-dimensional nanographene, 1% fluorine-modified polyacrylate copolymer, and 2% glass powder;
[0054] The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 7.8% benzyl alcohol, 10% salicylic acid, 10% phenalkamine, 8% epoxy resin, and 64.2% phenolic modified polyamide.
[0055] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reducing coating is the same as that of Example 4.
[0056] Example 6
[0057] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which, by weight ratio of 100%, consists of 87% of a paint component and 13% of a curing agent component;
[0058] The paint component is composed of the following raw materials according to a weight ratio of 100%: 72.8% epoxy resin, 0.5% glycidol, 2% hydrogenated castor oil, 0.5% polyamide wax, 15% red iron oxide, 3% two-dimensional carbon nanotubes, 2.2% two-dimensional nanographene, 1% fluorine-modified polyacrylate copolymer, and 3% glass powder;
[0059] The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 6% benzyl alcohol, 10% salicylic acid, 20% phenalkamine, 8% epoxy resin, and 56% phenolic modified polyamide.
[0060] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reducing coating is the same as that of Example 4.
[0061] Example 7
[0062] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which, by weight ratio of 100%, consists of 87% of a paint component and 13% of a curing agent component;
[0063] The paint component is composed of the following raw materials according to a weight ratio of 100%: 74% epoxy resin, 0.5% glycidol, 3% hydrogenated castor oil, 1% polyamide wax, 10% red iron oxide, 4% two-dimensional carbon nanotubes, 3% two-dimensional nanographene, 0.5% fluorine-modified polyacrylate copolymer, and 4% glass powder;
[0064] The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 7% benzyl alcohol, 8% salicylic acid, 25% phenalkamine, 12% epoxy resin, and 48% phenolic modified polyamide.
[0065] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reducing coating is the same as that of Example 4.
[0066] Example 8
[0067] A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, which, by weight ratio of 100%, consists of 87% of a paint component and 13% of a curing agent component;
[0068] The paint component is composed of the following raw materials according to a weight ratio of 100%: 74% epoxy resin, 0.2% glycidol, 3% hydrogenated castor oil, 1% polyamide wax, 13% red iron oxide, 4% two-dimensional carbon nanotubes, 2.7% two-dimensional nanographene, 0.1% fluorine-modified polyacrylate copolymer, and 2% glass powder;
[0069] The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 6% benzyl alcohol, 8% salicylic acid, 24% phenalkamine, 10% epoxy resin, and 52% phenolic modified polyamide.
[0070] The preparation method of the two-dimensional nano-modified solvent-free epoxy internal drag reducing coating is the same as that of Example 4.
[0071] Performance Testing
[0072] The coatings obtained in Example 1, Example 4 and Example 6 were tested for performance. The specific testing methods and results are shown in Table 1.
[0073] Table 1 Test conditions and results
[0074]
Claims
1. A two-dimensional nano-modified solvent-free epoxy internal drag reduction coating, characterized in that: Based on a weight ratio of 100%, it is composed of 85-90% of paint components and 10-15% of curing agent components; The paint component is composed of the following raw materials at a weight ratio of 100%: Epoxy functional group active diluent 0.2-1%, hydrogenated castor oil 2-4%, polyamide wax 0.2-1%, pigment 8-35%, two-dimensional carbon nanotube 2-6%, two-dimensional nanographene 2-4%, fluorine-modified polyacrylate copolymer 0.1-1%, glass powder 1-5%, and the balance is epoxy resin; The curing agent component is composed of the following raw materials based on a weight ratio of 100%: 3-8% benzyl alcohol, 2-10% salicylic acid, 10-30% phenalkamine, 5-20% epoxy resin, and the balance is phenolic modified polyamide.
2. According to claim 1, the two-dimensional nano-modified solvent-free epoxy internal drag reduction coating is characterized in that: The epoxy functional group active diluent is glycidol.
3. The two-dimensional nano-modified solvent-free epoxy internal drag reduction coating according to claim 2, characterized in that: The pigment is red iron oxide.
4. The two-dimensional nano-modified solvent-free epoxy internal drag reduction coating according to claim 3, characterized in that: The paint component is composed of the following raw materials: Epoxy functional group active diluent 0.2-1%, hydrogenated castor oil 2-4%, polyamide wax 0.2-1%, pigment 8-25%, two-dimensional carbon nanotube 3-5%, two-dimensional nanographene 2-3.8%, fluorine-modified polyacrylate copolymer 0.1-1%, glass powder 1-5%, and the balance is epoxy resin; The curing agent component is composed of the following raw materials: 3-7.8% benzyl alcohol, 2-10% salicylic acid, 10-28% phenalkamine, 8-17% epoxy resin, and the balance is phenolic modified polyamide.
5. The two-dimensional nano-modified solvent-free epoxy internal drag reduction coating according to claim 4, characterized in that: The paint component is composed of the following raw materials: Epoxy functional group active diluent 0.2-0.5%, hydrogenated castor oil 2-3%, polyamide wax 0.5-1%, pigment 10-15%, two-dimensional carbon nanotube 3-4%, two-dimensional nanographene 2.2-3%, fluorine-modified polyacrylate copolymer 0.1-1%, glass powder 2-4%, and the balance is epoxy resin; The curing agent component is composed of the following raw materials: 6-7% benzyl alcohol, 8-10% salicylic acid, 20-25% phenalkamine, 8-12% epoxy resin, and the balance is phenolic modified polyamide.
6. The method for preparing the two-dimensional nano-modified solvent-free epoxy internal drag reduction coating according to claim 1, characterized in that: The following steps are involved: (1) Preparing a paint component: mixing epoxy resin, epoxy functional group active diluent, hydrogenated castor oil, and polyamide wax, stirring until uniformly dispersed, and then sequentially adding pigment, two-dimensional carbon nanotubes, two-dimensional nanographene, fluorine-modified polyacrylate copolymer, and glass powder thereto, stirring until uniformly dispersed, to obtain a paint component; (2) preparing a curing agent component: mixing benzyl alcohol, salicylic acid, phenolic amine and epoxy resin under stirring, keeping the mixture at 90-100° C. for 3-5 hours, then adding phenolic modified polyamide thereto, stirring for 5-10 minutes, and obtaining a curing agent component; (3) Preparing coating: mixing the paint component and the curing agent component according to a certain proportion.