Lead alloy and its manufacturing method and application
By reducing the tin element content and adding an appropriate amount of selenium to the lead alloy, combined with the continuous rolling and rolling process of the tape casting machine, the corrosion resistance and floating charging life of the lead-acid battery are improved, and the complexity and cost of the existing lead alloy manufacturing process are solved. Higher problems achieve a more efficient production process.
Patent Information
- Application Number
- CN202310212227.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-07
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-03-07
AI Technical Summary
The existing lead alloy manufacturing process is complex and has high cost, resulting in insufficient corrosion resistance and floating charging life of lead-acid batteries.
The tin content in the lead alloy composition is 0 wt % to 0.2 wt %, the selenium content is 0.01 wt % to 0.03 wt %, and the balance is lead. The lead strip is made by continuous rolling and rolling by a tape casting machine, which is used to make lead acid The electrode plate grid of the battery is coated with lead paste through a curing process.
The tin element content in the lead alloy is reduced, the corrosion resistance and floating charging life of lead-acid batteries are improved, while simplifying the production process and reducing costs.
Smart Images

Figure CN116574938B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lead-acid battery production, and in particular relates to a lead alloy and a manufacturing method and application thereof. Background Art
[0002] Lead-acid batteries have the following characteristics: high voltage, low cost, good high-rate discharge performance, good high and low temperature resistance, easy floating charge, high safety, etc. Therefore, lead-acid batteries are widely used in lighting, starting, energy storage, communication backup power supply and other fields.
[0003] In the prior art, the physical and chemical properties of lead alloys can be improved by adding a small amount of other metals. Currently, the types of alloys used in lead-acid battery grids include rare earth alloys, lead-tin alloys, lead-calcium alloys, lead-antimony alloys, etc.
[0004] Although the above-mentioned lead alloys can improve the performance of the motor grid after manufacture, these lead alloys contain three or even more components, and the relationship between the component contents is more complicated. Different elements are usually added through different steps during the manufacturing process to ensure that the element content in the manufactured alloy meets the standards, making the manufacturing process more complicated; and the addition of different types of elements increases the manufacturing cost of the electrode. Summary of the invention
[0005] The present invention aims at solving the problems in the prior art and proposes the following technical solutions:
[0006] The present invention provides a lead alloy, which includes the following components:
[0007] Tin 0wt%~0.2wt%;
[0008] Selenium 0.01wt% to 0.03wt%;
[0009] The balance is lead;
[0010] In addition, it should be noted that the present invention has certain requirements on the purity of the component elements. Lead is electrolytic lead with a purity of not less than 99.996%, and the other impurities are Ag≤8ppm; Cu≤10ppm; Sb≤7ppm; Sn≤5ppm; As≤5ppm; Bi≤40ppm; Fe≤5ppm; Ni≤2ppm; Cd≤2ppm; Zn≤4ppm; and the total impurities are ≤40ppm.
[0011] On the basis of the above-mentioned lead alloy, the present invention further provides a grid, which is made of a lead strip made of the above-mentioned lead alloy according to a grid stamping process.
[0012] The present invention also provides an electrode, the grid of which is made of the lead alloy mentioned above, and the outside of which is coated with lead paste through a curing process.
[0013] The present invention also provides a lead-acid storage battery, the positive and negative electrodes of the lead-acid storage battery are both made of the above-mentioned electrodes.
[0014] The lead alloy is prepared by the following method: each component of the lead alloy is configured in proportion, then mixed, smelted, and then continuously rolled into a lead strip by a strip casting machine. Specifically:
[0015] The thickness of the original lead strip is 12.5mm, among which the rolling ratios of the positive grid lead strip are 9.000mm, 6.000mm, 3.600mm, 2.4000mm, 1.800mm, 1.400mm, and 1.200mm respectively; the rolling ratios of the negative grid lead strip are 8.500mm, 5.350mm, 3.200mm, 2.100mm, 1.350mm, 1.100mm, and 0.900mm respectively.
[0016] The beneficial effects of the present invention are as follows: the present invention reduces the tin content in the lead alloy on the basis of the currently widely used alloy, improves the corrosion resistance of the alloy, and at the same time, the lead-acid battery made using the lead alloy exhibits an excellent floating charge life, and can also reduce production costs and simplify production processes. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Shown are the performance test results of high temperature floating charge of the lead-acid battery prepared in the embodiment. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the embodiments of the present invention more clear, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments.
[0019] The present invention provides a lead alloy, which includes the following components:
[0020] Tin 0wt%~0.2wt%;
[0021] Selenium 0.01wt% to 0.03wt%;
[0022] The balance is lead;
[0023] In addition, it should be noted that the present invention has certain requirements on the purity of the component elements. Lead is electrolytic lead with a purity of not less than 99.996%. It also includes some inevitable impurities, among which: Ag≤8ppm; Cu≤10ppm; Sb≤7ppm; Sn≤5ppm; As≤5ppm; Bi≤40ppm; Fe≤5ppm; Ni≤2ppm; Cd≤2ppm; Zn≤4ppm; the total impurities are ≤40ppm.
[0024] The manufacturing method of the lead alloy of the present invention is: each component of the lead alloy is configured in proportion, then mixed, smelted and then continuously rolled into a lead strip by a strip casting machine. In addition, the continuous rolling parameters are controlled according to the difference between positive and negative electrodes:
[0025] The thickness of the original lead strip is 12.5mm, among which the rolling ratios of the positive grid lead strip are 9.000mm, 6.000mm, 3.600mm, 2.4000mm, 1.800mm, 1.400mm, and 1.200mm respectively; the rolling ratios of the negative grid lead strip are 8.500mm, 5.350mm, 3.200mm, 2.100mm, 1.350mm, 1.100mm, and 0.900mm respectively.
[0026] The lead alloy of the present invention is mainly used for manufacturing electrode grids of lead-acid batteries.
[0027] The main content of the present invention is lead, which exceeds 99.5%, and only trace amounts of selenium and tin are added, which has a very significant effect on improving the performance of lead alloy as an electrode grid.
[0028] Examples 1 to 7
[0029] Considering the effect of the tin content in the lead-tin alloy on the performance of the lead-tin alloy, different embodiments with a gradual increase in the tin element are set to explore the performance of the lead-tin alloy, mainly the corrosion resistance and discharge performance.
[0030] Table 1 shows the weight percentage of each component in the lead-tin alloy.
[0031]
[0032] Table 1
[0033] Considering that too high Sn content in lead-tin alloy will lead to excessive hydrogen evolution at the electrode and increase electrode corrosion, the Sn content does not exceed 2%. The above components also include inevitable impurities.
[0034] Constant pressure corrosion tests were performed on Examples 1 to 7. The results are shown in Table 2.
[0035]
[0036] Table 2
[0037] Combining the data in Tables 1 and 2, it can be seen that within the range of Sn content not exceeding 2%, as the Sn content increases, the corrosion rate and corrosion depth show a downward trend. In other words, within this range, the corrosion resistance of lead-tin alloy as a plate can be improved by adding Sn.
[0038] Embodiments 8 to 28
[0039] The inventors made further adjustments based on the components of the lead-tin alloy, added selenium, set a gradient increase in the selenium element, and explored the performance of the lead-tin alloy in the three-component system.
[0040] Table 3 shows the weight percentage of each component in the lead-tin alloy, which also includes inevitable impurities.
[0041]
[0042]
[0043] Table 3
[0044] Constant pressure corrosion tests were performed on Examples 8 to 28. The results are shown in Table 4.
[0045]
[0046] Table 4
[0047] Combining the data in Tables 3 and 4, it can be seen that by adding selenium, the corrosion resistance of lead-tin alloy as a plate can be improved, and as the selenium content increases, the help for the corrosion resistance of lead-tin alloy as a plate is more obvious; however, the inventors found that when the tin content is as low as 0.1%, although the added selenium content is only 0.02%, the corrosion resistance of the results of the constant voltage corrosion test is extremely significant, but when the selenium content is increased to 0.04%, this significant corrosion resistance does not exist.
[0048] Embodiments 29 to 84
[0049] The tin content was controlled at 0-0.3%, and the selenium content was controlled at 0-0.04% to further explore the performance of the lead-tin alloy.
[0050] Table 5 shows the weight percentage of each component in the lead-tin alloy, which also includes inevitable impurities.
[0051]
[0052]
[0053] Table 5: Constant pressure corrosion test was carried out on Examples 8 to 28. The results are shown in Table 6.
[0054]
[0055]
[0056] Table 6
[0057] Combining the data in Tables 5 and 6, it can be seen that when the tin addition amount does not exceed 0.2% and the selenium addition amount does not exceed 0.03%, the resulting lead-tin alloy has relatively stable corrosion resistance.
[0058] In the present invention, the specific method of the constant voltage corrosion test is: the temperature is set at 60 ° C, the voltage is set at 2.27V, the constant voltage corrosion is performed for 1440 hours, and then the corrosion layer is stripped with a sugar-alkali solution to calculate the corrosion rate. The corrosion results include: 60-day corrosion depth (unit: mm), corrosion rate (unit: mg / mc 2 h).
[0059] Electrode grids were prepared with 0.1% tin, 0.02% selenium and the balance lead, and further assembled into 12V 190Ah batteries. The high temperature floating charge performance test was performed on them. The test results are shown in Figure 1 The results show that its high-temperature float charge reaches more than 9 units and has an excellent float charge life.
[0060] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them.
Claims
1. Lead alloy, characterized in that It is composed of the following components: Tin 0.1wt%; Selenium 0.02wt%; The balance is lead, and the total amount of lead impurities is ≤40ppm.
2. A grid, characterized in that: The raw material of the grid is the lead alloy described in claim 1.
3. An electrode, characterized in that The electrode comprises the grid according to claim 2 and a lead paste solidified outside the grid.
4. A lead-acid battery, characterized in that: The positive / negative electrodes of the lead-acid battery are the electrodes according to claim 3.
5. A method for producing a lead alloy, characterized in that: The lead alloy is the lead alloy described in claim 1, and the manufacturing method is: configure the components of the lead alloy, melt them after mixing, and then continuously roll them into lead strips through a strip casting machine.
Citation Information
Patent Citations
Aluminum alloy and applications and production method of aluminum alloy
CN101555559A
Lead alloys for accumulators contg copper and tin - improved by addn of selenium or tellurium, and opt palladium and silver
DE2452842A1
Lead alloy for lead storage battery, and lead storage battery
JP2008266739A