Silicon-rich anti-reflective coating resin material and preparation method thereof

By using skeleton cyclosiloxane, light absorbing group and crosslinking group-containing cyclosiloxane, silicone rich antireflective coating resin, the problem of poor stability in the prior art is solved, and high stability and cost are achieved The reduced effect meets the optical parameter requirements of different application scenarios.

CN116589921BActive Publication Date: 2024-12-03QIANWAN INST OF CNITECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310535538.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-12-03
Estimated Expiration
2043-05-12

AI Technical Summary

Technical Problem

The existing silicon-rich anti-reflective coating has poor stability, resulting in self-polymerization reaction during storage, affecting the yield rate and cost efficiency of chip manufacturing.

Method used

Using skeleton cyclosiloxane, light absorbing group-containing cyclosiloxane and crosslinking group-containing cyclosiloxane as raw materials, silicon-rich antireflective coating resin is prepared by ring-opening polymerization to optimize molecular structure and improve stability sex.

Benefits of technology

It significantly improves the stability and shelf life of silicon-rich anti-reflective coatings, reduces storage costs, and achieves fine regulation of silicon content and optical parameters, meeting the etching rate and anti-reflective function requirements in different application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116589921B_ABST
    Figure CN116589921B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polymer materials, and specifically relates to a silicon-rich anti-reflective coating resin material and a preparation method thereof. The raw materials for preparing the silicon-rich anti-reflective coating resin material of the present invention include cyclosiloxane, cyclosiloxane containing a light-absorbing group, and cyclosiloxane containing a cross-linking group. The cyclosiloxane containing a light-absorbing group can control the optical parameters of the resin, and the cyclosiloxane containing a cross-linking group provides a cross-linking site. The prepared silicon-rich anti-reflective coating resin material can meet the requirements for the etching rate and anti-reflective function of the silicon-rich anti-reflective coating in different application scenarios.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a silicon-rich anti-reflective coating resin material and a preparation method thereof. Background Art

[0002] As the integration level of semiconductor components increases, the line width requirements of semiconductor components are getting smaller and smaller, and the control of critical dimensions is becoming more and more important. In order to prepare smaller and more sophisticated semiconductor devices, many new processes and materials have been introduced into the photolithography system. Among them, the depth of focus and aspect ratio limit the thickness of the photoresist. In some 45nm process technologies, the thickness of the photoresist is limited to 150nm, and it will become thinner and thinner with the update of technology. Such a thin imaging layer cannot provide sufficient plasma etching resistance, resulting in the failure of photolithography pattern transfer. Usually, in order to improve the etching resistance, hard mask technology is often used, so multi-layer photolithography technology came into being.

[0003] Multilayer lithography is usually achieved by alternating organic and inorganic layers, and the pattern transfer of the photoresist is achieved by selective plasma etching between different layers. Multilayer lithography can be achieved by chemical vapor deposition or spin coating or a combination of both. Due to its simplicity and feasibility, spin coating is usually used as one of the main means of industrial lithography.

[0004] Silicon-rich anti-reflective coating is an important component of the spin-coated three-layer structure in multi-layer lithography technology. The photoresist, silicon-rich anti-reflective coating and spin-coated carbon layer have large differences in different plasma rates, which improves the overall etching resistance of the three-layer structure. At the same time, the silicon-rich anti-reflective coating and the spin-coated carbon layer have an anti-reflective effect on ultraviolet light during the lithography process, effectively reducing the standing wave effect, swing effect and notch effect.

[0005] The molecular structure design of silicon-rich anti-reflective coatings should take into account the influence of multiple factors: (1) silicon content, which mainly affects the etching rate. As the silicon content increases, the fluorine plasma etching rate becomes faster and the oxygen plasma etching rate becomes slower. The higher the silicon content, the greater the improvement in overall anti-etching ability. (2) The refractive index n and absorption coefficient k of the silicon-rich anti-reflective coating should match the application scenarios such as the photolithography process to achieve a good phase shift, form subtractive interference, eliminate the reflected light of the substrate, and play an anti-reflection role. (3) The surface properties of the silicon-rich anti-reflective coating should match the photoresist to ensure good adhesion between the silicon-rich anti-reflective coating and the photoresist and avoid the collapse of the photoresist during the development process.

[0006] For silicon-rich anti-reflection coatings, how to adjust the n value and k value is a hot and difficult point in material research. According to the Lorentz-Lorenz equation, the relationship between the n value of polymer materials and the relevant parameters of the polymer material structure is as follows:

[0007]

[0008] Where n is the refractive index, ρ is the density, N A is Avogadro's constant, M w is the molecular weight, ɑ is the linear molecular polarizability, [R] is the molar refractive index, V 0 is the molecular molar volume. The n value reflects the attenuation of the propagation speed of light in the medium, which is related to the polarization degree of the molecular structure of the medium. The k value reflects the attenuation of the energy of light when it propagates in the medium.

[0009] The preparation of siloxane sol by sol method is the main method for preparing silicon-rich anti-reflective coating, and it is also the only commercial method that can be found. At present, the research and patents in the field of silicon-rich anti-reflective coating are also mainly carried out around the sol method (such as CN1902546A, CN103627316A, CN103228706A, CN104066804A, CN104159726A, etc.). Due to the poor stability of siloxane polymers prepared by the sol method, self-polymerization reaction is prone to occur during storage, and this process cannot be prevented. The rate of self-polymerization reaction can only be reduced by lowering the storage temperature, adding stabilizers, etc. The super-large polysiloxane molecules formed by the self-polymerization reaction will form gel particles, and the increase in particle content will reduce the film quality, thereby affecting the yield rate of the chip manufacturing lithography process, and seriously affecting the chip manufacturing cost and efficiency. Summary of the invention

[0010] The object of the present invention is to provide a silicon-rich anti-reflection coating resin material and a method for preparing the silicon-rich anti-reflection coating resin material in view of the deficiencies in the prior art.

[0011] The first object of the present invention is achieved by the following technical solutions:

[0012] A silicon-rich anti-reflection coating resin material, wherein the raw materials for preparing the silicon-rich anti-reflection coating resin material include skeleton cyclosiloxane, cyclosiloxane containing light-absorbing groups and cyclosiloxane containing cross-linking groups.

[0013] The silicon-rich anti-reflection coating resin material is prepared from raw materials including skeleton cyclosiloxane, cyclosiloxane containing light-absorbing groups and cyclosiloxane containing cross-linking groups.

[0014] Preferably, the light absorbing group includes one or more of phenyl, benzyl, naphthyl, anthracenyl, phenanthrenyl, pyrenyl, triphenylenyl, furanyl, pyridyl, and thienyl.

[0015] Preferably, the cross-linking group includes one or more of vinyl, acrylic, acrylate, crotonate and epoxy groups.

[0016] Preferably, the silicon-rich anti-reflective coating resin material comprises a polymer represented by formula (1):

[0017]

[0018] Among them, R 1 Including one or more of hydrogen, alkyl groups containing 1 to 8 carbon atoms, R 2 Including one or more of alkyl groups containing 1 to 8 carbon atoms; R 3 Including one or more of hydrogen, alkyl containing 1 to 8 carbon atoms, phenyl, R 4 Including one or more of phenyl, benzyl, naphthyl, anthracenyl, phenanthrenyl, pyrenyl, triphenylenyl, furanyl, pyridyl, thienyl; R 5 Including one or more of hydrogen, alkyl groups containing 1 to 8 carbon atoms, R 6 It includes one or more of vinyl, propenyl, acrylate, crotonate, and epoxy groups; x, y, and z are independently selected from 1 to 100.

[0019] The skeleton cyclosiloxane, the cyclosiloxane containing a light absorbing group and the cyclosiloxane containing a cross-linking group are used as raw materials for reacting to prepare a silicon-rich anti-reflective coating resin material. Preferably, the skeleton cyclosiloxane has a molecular formula shown in formula (2) after the reaction:

[0020]

[0021] Among them, R 1 Including one or more of hydrogen, alkyl groups containing 1 to 8 carbon atoms, R 2 One or more of an alkyl group containing 1 to 8 carbon atoms, wherein x is selected from 1 to 100;

[0022] Preferably, the cyclosiloxane containing a light-absorbing group has a molecular formula shown in formula (3) after reaction:

[0023]

[0024] Among them, R 3 Including one or more of hydrogen, alkyl containing 1 to 8 carbon atoms, phenyl, R 4 Including one or more of phenyl, benzyl, naphthyl, anthracenyl, phenanthrenyl, pyrenyl, triphenylenyl, furanyl, pyridyl, thienyl, y is selected from 1 to 100;

[0025] Preferably, the crosslinking group-containing cyclosiloxane has a molecular formula (4) after reaction:

[0026]

[0027] Among them, R 5Including one or more of hydrogen, alkyl groups containing 1 to 8 carbon atoms, R 6 It includes one or more of vinyl, acrylic, acrylate, crotonate and epoxy groups, and z is selected from 1 to 100.

[0028] Preferably, the skeleton cyclosiloxane includes but is not limited to one or more of trimethylcyclotrisiloxane, triethylcyclotrisiloxane, hexamethylcyclotrisiloxane, trimethyltriethylcyclotrisiloxane, hexaethylcyclotrisiloxane, tetramethylcyclotetrasiloxane, tetraethylcyclotetrasiloxane, octamethylcyclotetrasiloxane, tetramethyltetraethylcyclotetrasiloxane, octaethylcyclotetrasiloxane, pentamethylcyclopentasiloxane, pentaethylcyclopentasiloxane, decamethylcyclopentasiloxane, pentamethylpentaethylcyclopentasiloxane and decaethylcyclopentasiloxane.

[0029] Preferably, the cyclosiloxane containing a light-absorbing group includes, but is not limited to, trimethyltriphenylcyclotrisiloxane, hexaphenylcyclotrisiloxane, trimethyltribenzylcyclotrisiloxane, trimethyltrinathylcyclotrisiloxane, trimethyltrianthrylcyclotrisiloxane, trimethyltriphenanthrenylcyclotrisiloxane, trimethyltripyrenylcyclotrisiloxane, trimethyltribenzophenanthrenylcyclotrisiloxane, trimethyltrifuranylcyclotrisiloxane, trimethyltrithienylcyclotrisiloxane, trimethyltripyridylcyclotrisiloxane, tetramethyltetraphenylcyclotetrasiloxane, octaphenylcyclotetrasiloxane, tetramethyltetrabenzylcyclotetrasiloxane, tetramethyltetranaphthylcyclotetrasiloxane, tetramethyltetraanthrylcyclotetrasiloxane, tetramethyl The invention can be selected from the group consisting of pentamethyltetraphenanthrenylcyclotetrasiloxane, tetramethyltetrapyrenylcyclotetrasiloxane, tetramethyltetrabenzophenanthrenylcyclotetrasiloxane, tetramethyltetrafuranylcyclotetrasiloxane, tetramethyltetrathienylcyclotetrasiloxane, tetramethyltetrapyridylcyclotetrasiloxane, pentamethylpentaphenylcyclopentasiloxane, decaphenylcyclopentasiloxane, pentamethylpentabenzylcyclopentasiloxane, pentamethylpentanaphthylcyclopentasiloxane, pentamethylpentanthracenylcyclopentasiloxane, pentamethylpentaphenanthrenylcyclopentasiloxane, pentamethylpentapyrenylcyclopentasiloxane, pentamethylpentabenzophenanthrenylcyclopentasiloxane, pentamethylpentafen ...

[0030] Preferably, the cyclosiloxane containing a crosslinking group includes, but is not limited to, one or more of the compounds represented by formula (5) to (37):

[0031]

[0032]

[0033]

[0034]

[0035] Preferably, the preparation process of the silicon-rich anti-reflective coating resin material includes preparing raw materials and catalysts.

[0036] Preferably, the preparation process of the silicon-rich anti-reflective coating resin material also includes a solvent.

[0037] Preferably, in the preparation process of the silicon-rich anti-reflective coating resin material, the raw materials are dissolved in a solvent, and then a catalyst is added and heated to react.

[0038] Another object of the present invention is achieved by the following technical solutions:

[0039] A method for preparing a silicon-rich anti-reflective coating resin material comprises the following steps:

[0040] The skeleton cyclosiloxane, the cyclosiloxane containing the light absorbing group and the cyclosiloxane containing the cross-linking group are dissolved in a solvent, and then a catalyst is added, heated for reaction, and the silicon-rich anti-reflection coating resin material is obtained after separation and impurity removal.

[0041] Preferably, the molar ratio of the skeleton cyclosiloxane, the cyclosiloxane containing the light absorbing group and the cyclosiloxane containing the crosslinking group is 1: (0.01-0.5): (0.01-0.5). The molar ratio is determined according to the silicon content and optical parameter data of the silicon-rich anti-reflective coating, and the requirements for the silicon content and optical parameters of the silicon-rich anti-reflective coating in the application scenario are met. The molar ratio of the skeleton cyclosiloxane, the cyclosiloxane containing the light absorbing group and the cyclosiloxane containing the crosslinking group also determines the ratio of x, y and z in the general formula (1).

[0042] Preferably, the solvent includes but is not limited to pentane, hexane, heptane, octane, benzene, toluene, xylene, acetone, methanol, ethanol, butanol, ethylene glycol butyl ether, diethylene glycol butyl ether, triethylene glycol butyl ether, tetraethylene glycol butyl ether, ethylene glycol hexyl ether, diethylene glycol hexyl ether, diethylene glycol-2-ethylhexyl ether, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, 2-methoxyethyl acetate, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, propylene glycol methyl One or more of ether acetate, propylene glycol ethyl ether acetate, propylene glycol-1,2-dimethyl ether, propylene glycol diacetate, methyl methoxy acetate, dimethyl ketone, cyclohexanone, diisobutyl ketone, ethyl acetate, butyl acetate, 2-methylpropyl acetate, 3-methylbutyl acetate, ethyl lactate, methyl 3-methoxypropionate, cyclopentyl methyl ether, 4-hydroxy-4-methyl-2-pentanone, 3,5,5-trimethyl-1-hexanol, diethyl ether, dibutyl ether, tetrahydrofuran, dichloromethane, chloroform, and carbon tetrachloride.

[0043] Preferably, the catalyst comprises one or more of a basic catalyst and an acidic catalyst.

[0044] Further preferably, the catalyst includes but is not limited to one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide, cesium hydroxide, sodium methoxide, potassium methoxide, sodium ethoxide, potassium ethoxide, sodium isopropoxide, potassium isopropoxide, sodium tert-butoxide, potassium tert-butoxide, sodium trimethylsiliconate, potassium trimethylsiliconate, sodium phenyldimethylsiliconate, potassium phenyldimethylsiliconate, tetramethylammonium hydroxide, ethyltrimethylammonium hydroxide, phenyltrimethylammonium hydroxide, benzyltrimethylammonium hydroxide, tetraethylammonium hydroxide, methyltriethylammonium hydroxide, phenyltriethylammonium hydroxide, benzyltriethylammonium hydroxide, tetrapropylammonium hydroxide, phenyltripropylammonium hydroxide, benzyltripropylammonium hydroxide, tetrabutylammonium hydroxide, phenyltributylammonium hydroxide, benzyltributylammonium hydroxide, tetrahexylammonium hydroxide, sulfuric acid, hydrochloric acid, nitric acid, perchloric acid, and trifluoromethanesulfonic acid.

[0045] Preferably, the temperature of the heating reaction is 20 to 150° C., for example, it can be 20, 30, 40, 50, 60, 70, 90, 100, 120 or 150° C., but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. The time of the heating reaction is 5 min to 24 h, for example, it can be 5 min, 10 min, 20 min, 30 min, 40 min, 1 h, 2 h, 5 h, 10 h, 15 h, 20 h or 24 h, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0046] Preferably, the step of separating and removing impurities comprises reduced pressure distillation, wherein the pressure of the reduced pressure distillation is 1 to 20 mmHg and the temperature is 20 to 100°C.

[0047] The parameter control in the above preparation process is to ensure that the ring-opening polymerization reaction proceeds to an appropriate degree of polymerization, and the coating obtained after spin coating and baking of the prepared silicon-rich anti-reflective coating resin can ensure that the silicon content and optical parameters of the silicon-rich anti-reflective coating in the application scenario are met.

[0048] Compared with the prior art, the present invention has the following beneficial effects:

[0049] 1. The present invention uses skeleton cyclosiloxane, cyclosiloxane containing light-absorbing groups and cyclosiloxane containing crosslinking groups as preparation raw materials, and prepares silicon-rich anti-reflective coating resin by ring-opening polymerization, optimizes the molecular structure of polysiloxane, effectively improves the stability of the resin while meeting the full regulation of optical parameters, greatly improves the shelf life of the silicon-rich anti-reflective coating product, and reduces the storage cost of the silicon-rich anti-reflective coating product;

[0050] 2. The present invention can achieve fine control of the silicon content and optical parameters of the silicon-rich anti-reflection coating to meet the requirements of the etching rate and anti-reflection function of the silicon-rich anti-reflection coating in different application scenarios;

[0051] 3. The present invention is the first to use skeleton cyclosiloxane, cyclosiloxane containing light-absorbing groups and cyclosiloxane containing cross-linking groups as raw materials to prepare silicon-rich anti-reflective coating resins, providing a new direction for the preparation of silicon-rich anti-reflective coating resins. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 is an infrared spectrum of the silicon-rich anti-reflective coating resin in Example 1 of the present invention;

[0053] Figure 2 is a hydrogen nuclear magnetic resonance spectrum of the silicon-rich anti-reflective coating resin in Example 1 of the present invention;

[0054] Figure 3 This is an optical photograph of the silicon-rich anti-reflection coating in Application Example 1 of the present invention. DETAILED DESCRIPTION

[0055] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not intended for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosure of the present invention and do not have a limiting effect on the scope of protection. If not otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0056] Example 1

[0057] The preparation method of the silicon-rich anti-reflective coating resin material of this embodiment is as follows:

[0058] In a 500mL reactor, 200g of ethyl acetate, 86.6g of tetramethylcyclotetrasiloxane, 10.9g of tetramethyltetraphenylcyclotetrasiloxane, 6.9g of tetramethyltetra-3-glycidyloxypropylcyclotetrasiloxane and 2g of 98% sulfuric acid were added and stirred for reaction at a temperature of 30°C for 30min. After the reaction was completed, the silicon-rich anti-reflective coating resin material was separated by reduced pressure distillation (pressure 10mmHg, temperature 25°C).

[0059] Figure 1 is the infrared spectrum of the silicon-rich anti-reflection coating resin prepared in Example 1. It can be seen from the figure that 2960cm -1 The peak of CH stretching vibration is 1600 cm -1 The peak at 1450cm is the stretching vibration peak of the benzene ring skeleton. -1The peak of CH bending vibration is 1080cm -1 The Si-O-Si absorption peak is at 800 cm -1 The absorption peak is Si-C. Figure 2 The nuclear magnetic resonance hydrogen spectrum of the silicon-rich anti-reflective coating resin prepared in Example 1 shows that 7.2-7.7 ppm is the characteristic peak of the hydrogen atom of the benzene ring, 4.7 ppm is the characteristic peak of Si-H, 1.5-3.8 ppm is the absorption peak of the hydrogen atom in 3-glycidyloxypropyl, and 0.24 ppm is the absorption peak of Si-CH 3 characteristic peaks.

[0060] Example 2

[0061] The only difference from Example 1 is that 89.5 g of tetramethylcyclotetrasiloxane and 4.4 g of tetramethyltetraphenylcyclotetrasiloxane are added in Example 2, and the rest is the same as Example 1. For further explanation, the preparation method of the silicon-rich anti-reflective coating resin material of Example 2 is as follows:

[0062] In a 500mL reactor, 200g of ethyl acetate, 89.5g of tetramethylcyclotetrasiloxane, 4.4g of tetramethyltetraphenylcyclotetrasiloxane, 6.9g of tetramethyltetra-3-glycidyloxypropylcyclotetrasiloxane and 2g of 98% sulfuric acid were added, and the reaction was stirred at a temperature of 30°C and a reaction time of 30min. The silicon-rich anti-reflective coating resin material was separated by reduced pressure distillation (pressure 10mmHg, temperature 25°C).

[0063] Example 3

[0064] The only difference from Example 1 is that 81.8 g of tetramethylcyclotetrasiloxane and 21.8 g of tetramethyltetraphenylcyclotetrasiloxane are added in Example 3, and the rest is the same as Example 1. For further explanation, the preparation method of the silicon-rich anti-reflective coating resin material of Example 3 is as follows:

[0065] In a 500mL reactor, 200g of ethyl acetate, 81.8g of tetramethylcyclotetrasiloxane, 21.8g of tetramethyltetraphenylcyclotetrasiloxane, 6.9g of tetramethyltetra-3-glycidyloxypropylcyclotetrasiloxane and 2g of 98% sulfuric acid were added, and the reaction was stirred at a temperature of 30°C and a reaction time of 30min. The silicon-rich anti-reflective coating resin material was separated by reduced pressure distillation (pressure 10mmHg, temperature 25°C).

[0066] Example 4

[0067] The only difference from Example 1 is that 72.2 g of tetramethylcyclotetrasiloxane and 43.6 g of tetramethyltetraphenylcyclotetrasiloxane are added in Example 4, and the rest is the same as Example 1. For further explanation, the preparation method of the silicon-rich anti-reflective coating resin material of Example 4 is as follows:

[0068] In a 500mL reactor, 200g of ethyl acetate, 72.2g of tetramethylcyclotetrasiloxane, 43.6g of tetramethyltetraphenylcyclotetrasiloxane, 6.9g of tetramethyltetra-3-glycidyloxypropylcyclotetrasiloxane and 2g of 98% sulfuric acid were added, and the reaction was stirred at a temperature of 30°C and a reaction time of 30min. The silicon-rich anti-reflective coating resin material was separated by reduced pressure distillation (pressure 10mmHg, temperature 25°C).

[0069] Example 5

[0070] The only difference from Example 1 is that 12.0 g of tetramethyltetrabenzylcyclotetrasiloxane is added in Example 5 instead of tetramethyltetraphenylcyclotetrasiloxane, and the rest is the same as Example 1. For further explanation, the preparation method of the silicon-rich anti-reflective coating resin material of Example 5 is as follows:

[0071] In a 500mL reactor, 200g of ethyl acetate, 86.6g of tetramethylcyclotetrasiloxane, 12.0g of tetramethyltetrabenzylcyclotetrasiloxane, 6.9g of tetramethyltetra-3-glycidyloxypropylcyclotetrasiloxane and 2g of 98% sulfuric acid were added, and the reaction was stirred at a temperature of 30°C and a reaction time of 30min. The silicon-rich anti-reflective coating resin material was separated by reduced pressure distillation (pressure 10mmHg, temperature 25°C).

[0072] Example 6

[0073] The only difference from Example 1 is that 14.9 g of tetramethyltetranaphthylcyclotetrasiloxane is added in Example 6 instead of tetramethyltetraphenylcyclotetrasiloxane, and the rest is the same as Example 1. For further explanation, the preparation method of the silicon-rich anti-reflective coating resin material of Example 6 is as follows:

[0074] In a 500mL reactor, 200g of ethyl acetate, 86.6g of tetramethylcyclotetrasiloxane, 14.9g of tetramethyltetranaphthylcyclotetrasiloxane, 6.9g of tetramethyltetra-3-glycidyloxypropylcyclotetrasiloxane and 2g of 98% sulfuric acid were added, and the reaction was stirred at a temperature of 30°C and a reaction time of 30min. The silicon-rich anti-reflective coating resin material was separated by reduced pressure distillation (pressure 10mmHg, temperature 25°C).

[0075] Example 7

[0076] The only difference from Example 1 is that 11.4 g of tetramethyltetrathienylcyclotetrasiloxane is added in Example 7 instead of tetramethyltetraphenylcyclotetrasiloxane, and the rest is the same as Example 1. For further explanation, the preparation method of the silicon-rich anti-reflective coating resin material of Example 7 is as follows:

[0077] In a 500mL reactor, 200g of ethyl acetate, 86.6g of tetramethylcyclotetrasiloxane, 11.4g of tetramethyltetrathienylcyclotetrasiloxane, 6.9g of tetramethyltetra-3-glycidyloxypropylcyclotetrasiloxane and 2g of 98% sulfuric acid were added, and the reaction was stirred at a temperature of 30°C and a reaction time of 30min. The silicon-rich anti-reflective coating resin was separated by reduced pressure distillation (pressure 10mmHg, temperature 25°C).

[0078] Example 8

[0079] The preparation method of the silicon-rich anti-reflective coating resin material of this embodiment is as follows:

[0080] In a 500mL reactor, 200g of toluene, 86.6g of tetramethylcyclotetrasiloxane, 10.9g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetrapropylenecyclotetrasiloxane and 0.9g of tetramethylammonium hydroxide were added, and the reaction was stirred at 70°C for 10min. The silicon-rich anti-reflective coating resin was separated by reduced pressure distillation (pressure 10mmHg, temperature 25°C).

[0081] Example 9

[0082] The preparation method of the silicon-rich anti-reflective coating resin material of this embodiment is as follows:

[0083] In a 500mL reactor, 200g of toluene, 106.8g of tetraethylcyclotetrasiloxane, 10.9g of tetramethyltetraphenylcyclotetrasiloxane, 8g of tetramethyltetrapropylenecyclotetrasiloxane and 0.9g of tetramethylammonium hydroxide were added, and the mixture was stirred for reaction at 70°C for 10min. The silicon-rich anti-reflective coating resin was separated by reduced pressure distillation (pressure 10mmHg, temperature 50°C).

[0084] The silicon-rich anti-reflection coating resin materials of the above Examples 1-9 were subjected to gel chromatography analysis to obtain the molecular weight and molecular weight distribution, as shown in Table 1.

[0085] Table 1 Molecular weight and molecular weight distribution of silicon-rich anti-reflective coating resin materials of Examples 1-9

[0086]

[0087] Application Example 1

[0088] The silicon-rich anti-reflection coating resin material of Example 1 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 1. The silicon-rich anti-reflection coating sample 1 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 1-1.

[0089] Optical photo of silicon-rich anti-reflective coating Figure 3 shown.

[0090] The silicon-rich anti-reflection coating sample 1 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 1-2.

[0091] Application Example 2

[0092] The silicon-rich anti-reflection coating resin material of Example 2 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 2. The silicon-rich anti-reflection coating sample 2 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 2-1.

[0093] The silicon-rich anti-reflection coating sample 2 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 2-2.

[0094] Application Example 3

[0095] The silicon-rich anti-reflection coating resin material of Example 3 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 3. The silicon-rich anti-reflection coating sample 3 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 3.

[0096] The silicon-rich anti-reflection coating sample 3 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 3-2.

[0097] Application Example 4

[0098] The silicon-rich anti-reflection coating resin material of Example 4 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 4. The silicon-rich anti-reflection coating sample 4 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 4.

[0099] The silicon-rich anti-reflection coating sample 4 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 4-2.

[0100] Application Example 5

[0101] The silicon-rich anti-reflection coating resin material of Example 5 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 5. The silicon-rich anti-reflection coating sample 5 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 5.

[0102] The silicon-rich anti-reflection coating sample 5 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 5-2.

[0103] Application Example 6

[0104] The silicon-rich anti-reflection coating resin material of Example 6 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 6. The silicon-rich anti-reflection coating sample 6 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 6.

[0105] The silicon-rich anti-reflection coating sample 6 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 6-2.

[0106] Application Example 7

[0107] The silicon-rich anti-reflection coating resin material of Example 7 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 7. The silicon-rich anti-reflection coating sample 7 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 7.

[0108] The silicon-rich anti-reflection coating sample 7 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 7-2.

[0109] Application Example 8

[0110] The silicon-rich anti-reflection coating resin material of Example 8 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 8. The silicon-rich anti-reflection coating sample 8 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 8.

[0111] The silicon-rich anti-reflection coating sample 8 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 8-2.

[0112] Application Example 9

[0113] The silicon-rich anti-reflection coating resin material of Example 9 was filtered using a PTFE filter membrane (pore size of 0.1 μm), and 0.5 g of the resin was dissolved in 9.5 g of propylene glycol ethyl ether solvent to obtain a silicon-rich anti-reflection coating sample 9. The silicon-rich anti-reflection coating sample 9 was spin-coated on a 2-inch silicon wafer and dried to obtain a silicon-rich anti-reflection coating 9.

[0114] The silicon-rich anti-reflection coating sample 9 was stored in a constant temperature box at 40° C. for 30 days, then spin-coated on a 2-inch silicon wafer and baked to obtain a silicon-rich anti-reflection coating 9-2.

[0115] The optical parameters of the silicon-rich anti-reflection coatings of the above application examples 1-9 were characterized at 193 nm to obtain n, k values ​​and film thickness, as shown in Table 2.

[0116] Table 2

[0117]

[0118]

[0119] FL1 is the thickness of the silicon-rich anti-reflection coating obtained by spin coating and drying the freshly prepared silicon-rich anti-reflection coating sample, and FL2 is the thickness of the silicon-rich anti-reflection coating obtained by spin coating and drying the silicon-rich anti-reflection coating sample after being stored in a constant temperature box at 40°C for 30 days. As can be seen from Table 2, the values ​​of FL2 and FL1 are similar, indicating that the silicon-rich anti-reflection coating sample has excellent storage stability and can still form a film layer of similar thickness after being stored at a higher temperature for 30 days.

[0120] In summary, the present invention uses cyclosiloxane, cyclosiloxane containing light absorbing groups and cyclosiloxane containing crosslinking groups as reaction monomers to prepare silicon-rich anti-reflective coating resin by ring-opening polymerization. This method improves the disadvantage of poor stability of the resin prepared by the sol method and fundamentally improves the storage stability of the silicon-rich anti-reflective coating resin. At the same time, the ratio of the three cyclosiloxanes directly controls the silicon content in the resin, the cyclosiloxane containing light absorbing groups can control the optical parameters of the resin, and the cyclosiloxane containing crosslinking groups provides crosslinking sites, which can meet the requirements for the etching rate and anti-reflective function of the silicon-rich anti-reflective coating in different application scenarios.

[0121] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0122] In the preparation method of the present invention, the order of each step is not limited to the order listed. For those skilled in the art, without creative work, the order of each step is also within the protection scope of the present invention. In addition, two or more steps or actions can be performed simultaneously.

[0123] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A silicon-rich anti-reflective coating resin material, characterized in that: The raw materials for preparing the silicon-rich anti-reflective coating resin material include skeleton cyclosiloxane, cyclosiloxane containing light-absorbing groups and cyclosiloxane containing cross-linking groups; The skeleton cyclosiloxane, the cyclosiloxane containing the light absorbing group and the cyclosiloxane containing the cross-linking group are dissolved in a solvent, and then a catalyst is added, heated for reaction, and the silicon-rich anti-reflective coating resin material is obtained after separation and impurity removal; The solvent includes pentane, hexane, heptane, octane, benzene, toluene, xylene, acetone, ethylene glycol butyl ether, diethylene glycol butyl ether, triethylene glycol butyl ether, tetraethylene glycol butyl ether, ethylene glycol hexyl ether, diethylene glycol hexyl ether, diethylene glycol-2-ethylhexyl ether, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, 2-methoxyethyl acetate, propylene glycol methyl ether, propylene glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, propylene glycol methyl ether. One or more of acetate, propylene glycol ethyl ether acetate, propylene glycol-1,2-dimethyl ether, propylene glycol diacetate, methyl methoxy acetate, dimethyl ketone, cyclohexanone, diisobutyl ketone, ethyl acetate, butyl acetate, 2-methylpropyl acetate, 3-methylbutyl acetate, ethyl lactate, methyl 3-methoxypropionate, cyclopentyl methyl ether, 4-hydroxy-4-methyl-2-pentanone, diethyl ether, dibutyl ether, tetrahydrofuran, dichloromethane, chloroform, and carbon tetrachloride; The catalyst comprises one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide, cesium hydroxide, sodium methoxide, potassium methoxide, sodium ethoxide, potassium ethoxide, sodium isopropoxide, potassium isopropoxide, sodium tert-butoxide, potassium tert-butoxide, sodium trimethylsiliconate, potassium trimethylsiliconate, sodium phenyldimethylsiliconate, potassium phenyldimethylsiliconate, tetramethylammonium hydroxide, ethyltrimethylammonium hydroxide, phenyltrimethylammonium hydroxide, benzyltrimethylammonium hydroxide, tetraethylammonium hydroxide, methyltriethylammonium hydroxide, phenyltriethylammonium hydroxide, benzyltriethylammonium hydroxide, tetrapropylammonium hydroxide, phenyltripropylammonium hydroxide, benzyltripropylammonium hydroxide, tetrabutylammonium hydroxide, phenyltributylammonium hydroxide, benzyltributylammonium hydroxide, tetrahexylammonium hydroxide, sulfuric acid, hydrochloric acid, nitric acid, perchloric acid, and trifluoromethanesulfonic acid; The silicon-rich anti-reflective coating resin material comprises a polymer represented by formula (1): Among them, R1 includes one or more of hydrogen and an alkyl group containing 1 to 8 carbon atoms, R2 includes one or more of an alkyl group containing 1 to 8 carbon atoms; R3 includes one or more of hydrogen, an alkyl group containing 1 to 8 carbon atoms, and a phenyl group; R4 includes one or more of a phenyl group, a benzyl group, a naphthyl group, an anthracenyl group, a phenanthrenyl group, a pyrenyl group, a triphenylenyl group, a furanyl group, a pyridyl group, and a thienyl group; R5 includes one or more of hydrogen and an alkyl group containing 1 to 8 carbon atoms, R6 includes one or more of a vinyl group, a propenyl group, an acrylate group, a crotonyl group, and an epoxy group; x, y, and z are independently selected from 1 to 100.

2. The silicon-rich anti-reflection coating resin material according to claim 1, characterized in that: The skeleton cyclosiloxane includes one or more of trimethylcyclotrisiloxane, triethylcyclotrisiloxane, hexamethylcyclotrisiloxane, trimethyltriethylcyclotrisiloxane, hexaethylcyclotrisiloxane, tetramethylcyclotetrasiloxane, tetraethylcyclotetrasiloxane, octamethylcyclotetrasiloxane, tetramethyltetraethylcyclotetrasiloxane, octaethylcyclotetrasiloxane, pentamethylcyclopentasiloxane, pentaethylcyclopentasiloxane, decamethylcyclopentasiloxane, pentamethylpentaethylcyclopentasiloxane, and decaethylcyclopentasiloxane.

3. The silicon-rich anti-reflection coating resin material according to claim 1, characterized in that: The cyclosiloxane containing the light absorbing group includes trimethyl triphenyl cyclotrisiloxane, hexaphenyl cyclotrisiloxane, trimethyl tripenzyl cyclotrisiloxane, trimethyl trinaphthyl cyclotrisiloxane, trimethyl trianthryl cyclotrisiloxane, trimethyl triphenanthryl cyclotrisiloxane, trimethyl tripyrenyl cyclotrisiloxane, trimethyl tribenzophenanthryl cyclotrisiloxane, trimethyl trifuranyl cyclotrisiloxane, trimethyl trithienyl cyclotrisiloxane, trimethyl tripyridyl cyclotrisiloxane, tetramethyl tetraphenyl cyclotetrasiloxane, octaphenyl cyclotetrasiloxane, tetramethyl tetrabenzyl cyclotetrasiloxane, tetramethyl tetranaphthyl cyclotetrasiloxane, tetramethyl tetraanthryl cyclotetrasiloxane, tetramethyl tetraphenanthryl cyclotetrasiloxane, One or more of cyclotetrasiloxane, tetramethyltetrapyrenylcyclotetrasiloxane, tetramethyltetrabenzophenanthrylcyclotetrasiloxane, tetramethyltetrafuranylcyclotetrasiloxane, tetramethyltetrathienylcyclotetrasiloxane, tetramethyltetrapyridylcyclotetrasiloxane, pentamethylpentaphenylcyclopentasiloxane, decaphenylcyclopentasiloxane, pentamethylpentabenzylcyclopentasiloxane, pentamethylpentanaphthylcyclopentasiloxane, pentamethylpentanthracenylcyclopentasiloxane, pentamethylpentaphenanthrylcyclopentasiloxane, pentamethylpentapyrenylcyclopentasiloxane, pentamethylpentabenzophenanthrylcyclopentasiloxane, pentamethylpentafurylcyclopentasiloxane, pentamethylpentathienylcyclopentasiloxane and pentamethylpentapyridylcyclopentasiloxane.

4. The silicon-rich anti-reflection coating resin material according to claim 1, characterized in that: The crosslinking group-containing cyclosiloxane includes one or more compounds represented by formula (5) to (37):

5. The method for preparing a silicon-rich anti-reflective coating resin material according to claim 1, characterized in that: The following steps are involved: The skeleton cyclosiloxane, the cyclosiloxane containing the light absorbing group and the cyclosiloxane containing the cross-linking group are dissolved in a solvent, and then a catalyst is added, heated for reaction, and separated and impurities are removed to obtain a silicon-rich anti-reflective coating resin material; the solvent includes pentane, hexane, heptane, octane, benzene, toluene, xylene, acetone, ethylene glycol butyl ether, diethylene glycol butyl ether, triethylene glycol butyl ether, tetraethylene glycol butyl ether, ethylene glycol hexyl ether, diethylene glycol hexyl ether, diethylene glycol-2-ethylhexyl ether, ethylene glycol butyl ether acetate, diethylene glycol butyl ether acetate, 2-methoxyethyl acetate, propylene glycol methyl ether, propylene glycol butyl ... One or more of glycol ethyl ether, propylene glycol propyl ether, propylene glycol butyl ether, dipropylene glycol methyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether acetate, propylene glycol-1,2-dimethyl ether, propylene glycol diacetate, methyl methoxy acetate, dimethyl ketone, cyclohexanone, diisobutyl ketone, ethyl acetate, butyl acetate, 2-methylpropyl acetate, 3-methylbutyl acetate, ethyl lactate, methyl 3-methoxypropionate, cyclopentyl methyl ether, 4-hydroxy-4-methyl-2-pentanone, diethyl ether, dibutyl ether, tetrahydrofuran, dichloromethane, chloroform, and carbon tetrachloride; The catalyst includes one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide, cesium hydroxide, sodium methoxide, potassium methoxide, sodium ethoxide, potassium ethoxide, sodium isopropoxide, potassium isopropoxide, sodium tert-butoxide, potassium tert-butoxide, sodium trimethylsiliconate, potassium trimethylsiliconate, sodium phenyldimethylsiliconate, potassium phenyldimethylsiliconate, tetramethylammonium hydroxide, ethyltrimethylammonium hydroxide, phenyltrimethylammonium hydroxide, benzyltrimethylammonium hydroxide, tetraethylammonium hydroxide, methyltriethylammonium hydroxide, phenyltriethylammonium hydroxide, benzyltriethylammonium hydroxide, tetrapropylammonium hydroxide, phenyltripropylammonium hydroxide, benzyltripropylammonium hydroxide, tetrabutylammonium hydroxide, phenyltributylammonium hydroxide, benzyltributylammonium hydroxide, tetrahexylammonium hydroxide, sulfuric acid, hydrochloric acid, nitric acid, perchloric acid, and trifluoromethanesulfonic acid.

6. The preparation method according to claim 5, characterized in that: The temperature of the heating reaction is 20-150° C., and the time of the heating reaction is 5 min-24 h.