A method for synthesizing quantum dots by removing acid
By forming a low-boiling-point azeotrope between acid and solvent to extract acid during quantum dot synthesis, the method stabilizes the reaction, addressing fast reaction rates and low yield issues, achieving high-efficiency quantum dots.
Patent Information
- Application Number
- CN202310576026.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-05-18
AI Technical Summary
Existing quantum dot synthesis methods face issues with fast reaction rates, difficulty in mass production, and low quantum yield due to inadequate removal of acid generated during the synthesis process, which causes wavelength red shift.
A method involving the formation of a low-boiling-point azeotrope between the acid and an organic solvent under vacuum conditions to continuously extract the acid generated during synthesis, using the azeotropic principle to maintain a stable reaction environment.
This approach allows for the smooth progression of the reaction, resulting in quantum dots with high luminous efficiency by effectively removing the acid impact, thereby improving the synthesis process.
Smart Images

Figure CN116606651B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of quantum dot synthesis, and in particular to a method for synthesizing quantum dots by removing acid. Background Art
[0002] Quantum dots are a new type of nanomaterial. Common quantum dot materials include II-VI, III-V, I-III-VI, etc. Quantum dots themselves have the advantages of full color gamut display, narrow-band continuous spectrum, high color purity, strong color reproduction ability and excellent color rendering, and have the advantages of strong stability, long life, and not easy to age, and have a very broad application scenario.
[0003] The existing technology for preparing quantum dots has disadvantages such as too fast reaction rate, difficulty in mass production, and low quantum yield. The reason for this is that the acid generated during the synthesis process cannot be removed well. The residual acid will accelerate the reaction rate and cause the wavelength to red shift too quickly. Therefore, it is of great significance to develop a method to remove the acid generated during the synthesis of quantum dots. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a method for synthesizing quantum dots by removing acid.
[0005] The present invention solves the technical problem by adopting the following technical solutions.
[0006] The invention provides a method for synthesizing quantum dots by removing acid, comprising the following steps: in a vacuum exhaust state, heating a cationic precursor, an acid ligand and an organic solvent to 80-120° C., reacting for 20-30 minutes, and then heating to 150-180° C. and stirring for 10-20 minutes to obtain a reaction solution for preliminary removal of acid; then reacting the reaction solution with an anionic precursor at a first temperature to obtain nanoclusters, and then reacting the nanoclusters at a second temperature to obtain quantum dots.
[0007] The present invention provides a method for preparing core-shell quantum dots, comprising: preparing quantum dot cores by the above method, and then coating the quantum dot cores to obtain core-shell quantum dots.
[0008] The present invention has the following beneficial effects:
[0009] The present invention provides a method for synthesizing quantum dots by removing acid. The azeotropic principle is used to make the acid generated in the process of synthesizing quantum dots form a low-boiling-point azeotrope with an organic solvent. During the vacuum exhaust process, during the dissolution of raw materials and the subsequent reaction process, the acid generated in the system can be continuously extracted, so that the reaction proceeds smoothly and quantum dots with high luminous efficiency are obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0011] Figure 1 The absorption spectrum and emission spectrum of the quantum dots obtained in Example 1 for calculating QY. DETAILED DESCRIPTION
[0012] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0013] The following is a detailed description of a method for synthesizing quantum dots by removing acid provided in an embodiment of the present invention.
[0014] In the first aspect, an embodiment of the present invention provides a method for synthesizing quantum dots by acid removal, comprising the following steps: heating a cationic precursor, an acid ligand and an organic solvent to 80-120°C under a vacuum exhaust state, reacting for 20-30 minutes, and then heating to 150-180°C and stirring for 10-20 minutes to obtain a reaction solution for preliminary acid removal; then reacting the reaction solution with an anionic precursor at a first temperature to obtain nanoclusters, and then reacting the nanoclusters at a second temperature to obtain quantum dots.
[0015] The embodiment of the present invention provides a method for synthesizing quantum dots by removing acid. By using the azeotropic principle, when two liquids with similar properties are mixed, the solution formed is close to an ideal system. They dissolve in each other within a wide temperature range, and the vapor pressure conforms to Raoult's law. The azeotropic phenomenon is caused by the molecular structures of the components constituting the solution being different, which causes deviations from the ideal solution when mixed. If the vapor pressure of the solution deviates negatively from the ideal solution, that is, the activity coefficient is less than 1, the highest azeotrope is formed; if the vapor pressure of the solution deviates positively from the ideal solution, that is, the activity coefficient is greater than 1, the lowest azeotrope is formed, and the acid generated in the synthesis of quantum dots is more easily removed after forming an azeotrope with the organic solvent. Further, the method provided by the embodiment of the present invention, in the raw material dissolution stage and the reaction stage, the acid generated is extracted at a lower temperature by heating vacuum and Ar exhaust mode, and the acid is removed during the reaction process, which does not affect the reaction, but is conducive to the reaction, reduces the influence of the acid, and compared with the addition of acid removers, filtering and other methods, the method provided by the embodiment of the present invention is simple and efficient, does not need to stop the reaction, can be carried out continuously, and improves the success rate of quantum dot synthesis. Based on the above principle, the method provided by the embodiment of the present invention can make the acid generated in the quantum dot synthesis process form a low-boiling-point azeotrope with the organic solvent, and the acid can be easily removed to reduce the impact on the reaction, thereby improving the luminescence performance of the synthesized quantum dots.
[0016] In an optional embodiment, under vacuum exhaust, the cationic precursor, the acid ligand and the organic solvent are heated to 80-120° C. for reaction for 20-30 min, and then heated to 150-180° C. for stirring for 10-20 min to obtain a reaction solution with preliminary deacidification;
[0017] Preferably, under vacuum exhaust, the reaction is heated to 110° C. for 30 min, and then the temperature is raised to 170° C. and stirred for 30 min to completely dissolve the solid powder, thereby obtaining a reaction solution that is preliminarily deacidified and uniformly mixed;
[0018] More preferably, the exhaust gas is changed to Ar after the reaction solution is preliminarily deacidified by vacuuming for 60 minutes.
[0019] In an optional embodiment, the first temperature is 80-130°C;
[0020] Preferably, in the presence of Ar, the obtained reaction solution subjected to preliminary deacidification is cooled to 90° C., and then an anion precursor is introduced to react for 10 min to obtain nanoclusters.
[0021] In an optional embodiment, the first temperature is 80-130°C;
[0022] Preferably, after evacuating the air for 60 minutes, the exhaust gas is changed to Ar, the temperature is lowered to 90° C., and an anion precursor is injected to react for 10 minutes to form nanoclusters.
[0023] In an optional embodiment, the second temperature is 220-280°C;
[0024] Preferably, the nanoclusters are heated to 230° C. and reacted for 30 minutes to obtain quantum dots.
[0025] In an alternative embodiment, the acid ligand comprises one or more of undecylenic acid, dodecanoic acid, tetradecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid and stearic acid.
[0026] In an optional embodiment, the organic solvent includes one or more of toluene, carbon tetrachloride, n-octane, n-heptane, chlorobenzene, 1-bromobutane, 2-bromobutane, 1,2-dibromoethane and isopentyl chloride. The organic solvent selected above can form a low-boiling azeotrope with the acid generated during the synthesis of quantum dots, so that it can be removed by vacuuming and exhausting to reduce the effect of the acid on the reaction.
[0027] In an optional embodiment, the cationic precursor includes at least one of cadmium acetate, zinc chloride, zinc acetate, copper acetate, indium acetate, indium chloride, zinc chloride and lead chloride.
[0028] In an optional embodiment, the precursor of anionic phosphorus includes any one or more of tri(trimethylsilyl)phosphine, tri(triethylsilyl)phosphine, tri(triphenylsilyl)phosphine, tri(dimethylamino)phosphine and tri(diethylamino)phosphine.
[0029] In an optional embodiment, the molar ratio of the cationic precursor to the acid ligand is 1:2-6:1, and the molar ratio of the cationic precursor to the anionic phosphorus precursor is 1:5-1:1.
[0030] In a second aspect, an embodiment of the present invention provides a method for preparing core-shell quantum dots, comprising: preparing a quantum dot core by the above method, and then coating the quantum dot core to obtain a core-shell quantum dot.
[0031] In an optional embodiment, the quantum dot core is coated with ZnS, ZnSeS or ZnSe to obtain core-shell quantum dots.
[0032] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0033] Example 1
[0034] (1) In a three-necked flask equipped with a magnetic stirrer and an electric heating mantle, add 2.0 mmol In(Ac)3 (indium acetate), 1.0 mmol OA (oleic acid) and 6 mmol toluene, heat to 110°C under vacuum exhaust and react for 30 min, then heat to 180°C and stir for 10 min to completely dissolve the solid powder and mix the solution evenly;
[0035] (2) After evacuating the vacuum for 60 min, the exhaust gas was changed to Ar, the temperature was lowered to 90 °C, 3.2 mmol of tris(trimethylsilyl)phosphine was added and reacted for 10 min to form nanoclusters;
[0036] (3) The nanoclusters were then heated to 230 °C for 30 min to form quantum dot cores, which were then cleaned, coated with ZnSe and ZnS shells, and tested for absorption (UV) and emission (PL), see Figure 1 The maximum emission wavelength of the obtained quantum dots is 525.6 nm, and the calculated quantum efficiency is 95%.
[0037] Example 2
[0038] (1) In a three-necked flask equipped with a magnetic stirrer and an electric heating mantle, add 1.6 mmol In(Ac)3 (indium acetate), 5.0 mmol PA (palmitic acid) and 1.6 mmol n-octane, heat to 120°C under vacuum exhaust and react for 30 min, then heat to 170°C and stir for 10 min to completely dissolve the solid powder and mix the solution evenly;
[0039] (2) After evacuating the vacuum for 60 min, the exhaust gas was changed to Ar, the temperature was lowered to 80 °C, 4.5 mmol of tris(trimethylsilyl)phosphine was added and reacted for 10 min to form nanoclusters;
[0040] (3) The nanoclusters were then heated to 260°C for 30 min to form quantum dot cores, which were then cleaned and coated with ZnSe and ZnS shells. The absorption (UV) and emission (PL) of the cores were tested, and the quantum efficiency was calculated to be 92%.
[0041] Example 3
[0042] (1) In a three-necked flask equipped with a magnetic stirrer and an electric heating mantle, add 1.2 mmol Zn(Ac)2 (zinc acetate), 3.8 mmol LA (dodecanoic acid) and 2.4 mmol benzene, heat to 100°C under vacuum exhaust and react for 30 min, then heat to 180°C and stir for 20 min to completely dissolve the solid powder and mix the solution evenly;
[0043] (2) After evacuating the air for 60 min, the exhaust gas was changed to Ar, the temperature was lowered to 100 °C, 5.0 mmol of tri(diethylamino)phosphine was introduced and reacted for 10 min to form nanoclusters;
[0044] (3) The nanoclusters were then heated to 280°C for 30 min to form quantum dot cores, which were then cleaned and coated with ZnSe and ZnS shells. The absorption (UV) and emission (PL) of the cores were tested, and the quantum efficiency was calculated to be 88%.
[0045] Example 4
[0046] (1) In a three-necked flask equipped with a magnetic stirrer and an electric heating mantle, add 1.5 mmol InCl3 (indium chloride), 4.5 mmol OA (oleic acid) and 1.8 mmol carbon tetrachloride, heat to 80°C under vacuum exhaust and react for 30 min, then heat to 180°C and stir for 20 min to completely dissolve the solid powder and mix the solution evenly;
[0047] (2) After evacuating the vacuum for 60 min, the exhaust gas was changed to Ar, the temperature was lowered to 90 °C, 0.56 mmol of tris(trimethylsilyl)phosphine was added and reacted for 10 min to form nanoclusters;
[0048] (3) The nanoclusters were then heated to 240°C for 30 min to form quantum dot cores, which were then cleaned and coated with ZnSe and ZnS shells. The absorption (UV) and emission (PL) of the cores were tested, and the quantum efficiency was calculated to be 96%.
[0049] Example 5
[0050] (1) In a three-necked flask equipped with a magnetic stirrer and an electric heating mantle, add 1.8 mmol In(Ac)3 (indium acetate), 1.5 mmol LA (dodecanoic acid) and 1.8 mmol 1-bromobutane, heat to 100°C under vacuum exhaust and react for 30 min, then heat to 180°C and stir for 20 min to completely dissolve the solid powder and mix the solution evenly;
[0051] (2) After evacuating the vacuum for 60 min, the exhaust gas was changed to Ar, the temperature was lowered to 80 °C, 3.6 mmol of tris(trimethylsilyl)phosphine was added and reacted for 10 min to form nanoclusters;
[0052] (3) The nanoclusters were then heated to 230°C for 30 min to form quantum dot cores, which were then cleaned and coated with ZnSe and ZnS shells. The absorption (UV) and emission (PL) of the cores were tested, and the quantum efficiency was calculated to be 90%.
[0053] Comparative Example 1
[0054] The results of removing the acid by filtering or adding an acid scavenger are as follows: filtration is required in the middle of the reaction. Since quantum dots are easily oxidized, this method will not only reduce the quantum yield of quantum dots, but also prolong the reaction time. Using an acid scavenger to remove the acid will add other substances to the reaction system, which will also cause a decrease in the purity of the quantum dots.
[0055] Comparative Example 2
[0056] The steps are similar to those in Example 1, except that the temperature is raised to 110° C. under vacuum exhaust and reacted for 30 min, then raised to 130° C. and stirred. After the temperature is lowered, although the azeotrope formed by the acid produced during the reaction and the organic solvent can be removed, the raw materials cannot be completely dissolved due to the low temperature, resulting in insufficient and incomplete reaction.
[0057] Comparative Example 3
[0058] The steps are similar to those in Example 1, except that: heating to 110°C for 30 minutes, heating to 180°C for 10 minutes under vacuum exhaust, stirring to completely dissolve the solid powder, and mixing the solution evenly. The result is that the quality of the quantum dots is reduced. The reason is that during the synthesis of quantum dots, the reactants, intermediates, and products are all sensitive to water and air, and cannot exist stably in a water-oxygen environment. Therefore, it is necessary to evacuate and exhaust at the beginning of the reaction. On the one hand, the water and oxygen therein can be removed, and on the other hand, the acid generated during the reaction can be removed in time. If the reaction is not evacuated at the beginning, the reactants may not exist stably or other by-products may appear, affecting nucleation and the subsequent growth of quantum dots.
[0059] In summary, the embodiment of the present invention provides a method for synthesizing quantum dots by removing acid, comprising the following steps: in a vacuum exhaust state, heating a cationic precursor, an acid ligand and an organic solvent to 80-120°C for reaction for 20-30 minutes, and then heating to 150-180°C and stirring for 10-20 minutes to obtain a reaction solution for preliminary acid removal; then reacting the reaction solution with an anionic precursor at a first temperature to obtain nanoclusters, and then reacting the nanoclusters at a second temperature to obtain quantum dots. This method forms an azeotrope with the acid generated in the synthesis of quantum dots to better remove the acid generated in the synthesis of quantum dots, reduce the impact on the reaction, and has a beneficial effect on the synthesis of quantum dots.
[0060] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for synthesizing quantum dots by removing acid, It is characterized in that The following steps are involved: Under vacuum exhaust, the cationic precursor, the acid ligand and the organic solvent are heated to 80-120° C. for reaction for 20-30 minutes, and then the temperature is raised to 150-180° C. and stirred for 10-20 minutes to obtain a reaction solution with preliminary acid removal; the reaction solution is then reacted with the anionic precursor at a first temperature to obtain nanoclusters, and the nanoclusters are then reacted at a second temperature to obtain quantum dots; The acid ligand is selected from one or more of undecylenic acid, dodecanoic acid, tetradecanoic acid, hexadecanoic acid, octadecanoic acid, oleic acid and stearic acid; The organic solvent is selected from one or more of toluene, carbon tetrachloride, n-octane, n-heptane, chlorobenzene, 1-bromobutane, 2-bromobutane, 1,2-dibromoethane and chloroisopentane; The cationic precursor is selected from at least one of cadmium acetate, zinc chloride, zinc acetate, copper acetate, indium acetate, indium chloride, zinc chloride and lead chloride, and the anionic precursor is selected from any one or more of tris(trimethylsilyl)phosphine, tris(triethylsilyl)phosphine, tris(triphenylsilyl)phosphine, tris(dimethylamino)phosphine and tris(diethylamino)phosphine; The first temperature is 80-130°C, and the second temperature is 220-280°C.
2. The method according to claim 1, It is characterized in that The reaction solution was preliminarily deacidified by vacuuming for 60 min and then changed to Ar exhaust.
3. The method according to claim 2, It is characterized in that In the presence of Ar, the reaction solution obtained after preliminary deacidification was cooled to 90° C., and then the anion precursor was introduced to react for 10 minutes to obtain the nanoclusters.
4. The method according to claim 1, It is characterized in that The nanoclusters were heated to 230° C. and reacted for 30 minutes to obtain quantum dots.
5. The method according to claim 1, It is characterized in that The molar ratio of the cationic precursor to the acid ligand is 1:2-6:1, and the molar ratio of the cationic precursor to the anionic precursor is 1:5-1:
1.
6. A method for preparing core-shell quantum dots, It is characterized in that include: The quantum dot core is prepared by the method according to any one of claims 1 to 5, and then the quantum dot core is coated to obtain the core-shell quantum dot.
7. The preparation method according to claim 6, It is characterized in that The quantum dot core is coated with ZnS, ZnSeS or ZnSe to obtain the core-shell quantum dot.