A micro-lamellar structure reinforced silicon carbide ceramic composite material and preparation method thereof

By introducing microsheet structures and sintering aids into silicon carbide ceramics, the preparation of silicon carbide ceramics that densify and improve fracture toughness at lower temperatures is achieved, and the problems of material densification and low fracture toughness are solved. Good mechanical properties and high density.

CN116621584BActive Publication Date: 2024-11-15AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310749322.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-21
Publication Date
2024-11-15
Estimated Expiration
2043-06-21

AI Technical Summary

Technical Problem

Silicon carbide ceramic materials are difficult to achieve densification at lower temperatures, and their fracture toughness is low, limiting their widespread use.

Method used

The preparation method of enhanced silicon carbide ceramic composite material using microsheet structure is used to introduce graphene sheets and/or silicon carbide whiskers into silicon carbide powder, and use alumina, yttrium oxide, auxiliary oxide and boron powder as sintering The additive is subjected to high-pressure sintering below 1760°C to ensure uniform distribution of the microsheet structure and good mechanical properties.

Benefits of technology

The densification of silicon carbide ceramics is achieved at a lower temperature, which improves its fracture toughness and bending strength, and has a density of more than 98%, solving the problems of dispersion and high sintering temperature, and is suitable for a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004302131510000091
    Figure BDA0004302131510000091
  • Figure HDA0004302131520000011
    Figure HDA0004302131520000011
  • Figure HDA0004302131520000012
    Figure HDA0004302131520000012
Patent Text Reader

Abstract

The present invention relates to a micro-lamellar structure reinforced silicon carbide ceramic-based composite material and a preparation method thereof. The method uses silicon carbide as a matrix, silicon carbide whiskers and / or graphene sheets as reinforcements, adds dispersants and sintering aids, and achieves densification of silicon carbide ceramic composite materials at a relatively low temperature through hot pressing and spark plasma sintering. The specific preparation process is as follows: adding a coupling agent to ultrasonically disperse the micro-lamellar material, ball milling the dispersion liquid, silicon carbide powder and sintering aid, and performing a binder removal treatment on the ball-milled powder to obtain a composite material powder; hot pressing sintering or spark plasma sintering is adopted, and high-pressure instantaneous liquid phase sintering is adopted in a vacuum environment to obtain a high-performance silicon carbide composite material. The method achieves uniform dispersion of the micro-lamellar structure in the ceramic matrix by adding a dispersant, etc., and the added sintering aid and high pressure are used through high-pressure instantaneous liquid phase sintering to achieve densification of the silicon carbide ceramic composite material at a relatively low temperature, and has good mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic composite material preparation, and particularly relates to a micro-lamellar structure reinforced silicon carbide ceramic composite material and a preparation method thereof. Background Art

[0002] Silicon carbide (SiC) ceramics have high melting point, high strength, high hardness, high elastic modulus, good high temperature oxidation resistance, as well as radiation resistance, wear resistance and corrosion resistance. Dense silicon carbide-based ceramic composites are used in the aerospace field, nuclear reactor structural components, wear-resistant materials and high temperature structural materials. However, there are 88% covalent bonds and 12% ionic bonds between Si and C atoms in silicon carbide. Its strong covalent bonds and low diffusion coefficient at high temperature make it difficult to achieve densification of SiC ceramic-based materials through high temperature sintering. At the same time, the fracture toughness of silicon carbide ceramics is low. These two shortcomings limit the widespread application of silicon carbide ceramic-based materials. Therefore, how to achieve the densification of silicon carbide ceramics at a lower temperature and improve its fracture toughness is a key problem that needs to be solved urgently in silicon carbide ceramics.

[0003] At present, the introduction of the second phase layer structure toughening is an effective way to improve the strength and fracture toughness of silicon carbide ceramics. Silicon carbide whiskers, graphene layers and other structures can be pulled out, bridged and crack deflected through the layer structure, which is an ideal material for strengthening silicon carbide ceramic materials. On the other hand, adding sintering aids during the mixing process can significantly reduce the sintering temperature of silicon carbide ceramics and increase the driving force for densification.

[0004] However, the two lamellar structures of graphene and silicon carbide whiskers are prone to agglomeration and uneven dispersion during the mixing process with ceramic powders, which affects the density and performance of silicon carbide ceramic composites. Lee et al. (Lee, et al. Microstructure and Fracture Toughness of Hot-Pressed Silicon Carbide Reinforced with Silicon Carbide Whisker Journal of the American Ceramic Society, 1994, 77 (12), 3270-3272) prepared SiC whisker reinforced SiC ceramic composites by hot pressing sintering at 2000°C, but its fracture toughness was only 4 MPa·m 0.5, and too high a sintering temperature will cause the ceramic grains to grow, impair the mechanical properties, and may also destroy the silicon carbide whisker structure. Tonello (Tonello, et al. Fabrication and characterization of laminated SiC composites reinforced with graphene platelets, Materials Science and Engineering A 659 (2016) 158–164) used a pressureless sintering method to prepare graphene microplatelets reinforced silicon carbide composite ceramics at an extremely high temperature of 2200°C, but its flexural strength was only 300MPa and its density was about 97%. Therefore, problems such as the dispersion of microplatelet structures in SiC ceramics and excessively high sintering temperatures still exist, and the performance of ceramic materials needs to be further improved. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a micro-lamellar structure reinforced silicon carbide ceramic composite material and a preparation method thereof. The present invention toughens the lamellar structure. The ceramic composite material can evenly distribute the lamellar structure in the silicon carbide matrix structure, and form good mechanical properties with each other, and can achieve material densification at a relatively low temperature, which is conducive to application.

[0006] The present invention provides a method for preparing a micro-lamellar structure reinforced silicon carbide ceramic composite material, comprising the following steps:

[0007] Silicon carbide powder is used as raw material powder, and micro-lamellar material is used as reinforcement, wherein the micro-lamellar material is graphene sheet and / or silicon carbide whisker; aluminum oxide, yttrium oxide, auxiliary oxide and boron powder are used as sintering aids, wherein the auxiliary oxide is silicon dioxide and / or calcium oxide, and high-pressure sintering below 1760° C. is performed to obtain a micro-lamellar structure reinforced silicon carbide ceramic composite material.

[0008] Preferably, the silicon carbide powder has a particle size of 100 nm to 1 μm, more preferably 100 to 600 nm.

[0009] Preferably, the micro-sheet material has a sheet diameter cross-sectional height of 0.2 to 2 μm and a length of 5 to 20 μm; the micro-sheet material is preferably dispersed using a silane coupling agent.

[0010] Preferably, the preparation method comprises the following specific steps:

[0011] The micro-sheet material is dispersed in anhydrous ethanol to prepare a dispersion, and a silane coupling agent is selected as an additive;

[0012] The dispersion of the micro-sheet material is mixed with silicon carbide powder and a sintering aid, and ball milled;

[0013] The ball-milled powder is subjected to a binder removal treatment to obtain a composite material powder;

[0014] The composite material powder is sintered under high pressure at 1700° C. to 1760° C. to obtain a micro-lamellar structure reinforced silicon carbide ceramic composite material.

[0015] Preferably, in the mixed material, the content of micro-sheet material is 2-8wt%, the aluminum oxide, yttrium oxide and auxiliary oxide powders account for 5-9wt% in total, the boron powder accounts for 0.5-1wt%, and the balance is silicon carbide powder.

[0016] Preferably, the particle size of the boron powder is 1 to 3 μm, and the particle sizes of the aluminum oxide, yttrium oxide and auxiliary oxide powders are all 100 nm to 800 nm, more preferably 100 to 600 nm.

[0017] Preferably, the ball milling is planetary ball milling and is carried out in the presence of a dispersant; the amount of the dispersant used accounts for 0.5 to 1.5 wt % of the total amount of the powder.

[0018] Preferably, the planetary ball mill uses Si3N4 grinding balls, the ball-to-material ratio is 3-5:1, and the ball mill rotation speed is 100-200 rpm / min.

[0019] Preferably, the high-pressure sintering is carried out under vacuum conditions, first heating from room temperature to 1600°C at a heating rate of 10-100°C / min, then heating to 1700°C-1760°C at 5-15°C / min, and keeping warm for 20-60 minutes. During the sintering process, the axial sintering pressure is controlled to be 50-70MPa.

[0020] The present invention provides a micro-lamellar structure reinforced silicon carbide ceramic composite material obtained by the preparation method as described above, with a density of more than 98%.

[0021] Compared with the prior art, the specific preparation process of the silicon carbide ceramic composite material in the embodiment of the present invention includes: the micro-sheet material (graphene micro-sheets and / or silicon carbide whiskers) can be ultrasonically dispersed in anhydrous ethanol, preferably adding a coupling agent to disperse for 2 to 5 hours; the obtained dispersion liquid is planetarily ball milled with silicon carbide powder and a specific sintering aid, and the powder after ball milling is subjected to a binder removal treatment to obtain the powder of the silicon carbide composite material; hot pressing sintering or discharge plasma sintering at a relatively low temperature can be used, and high-pressure instantaneous liquid phase sintering in a vacuum environment can be used to obtain a high-performance silicon carbide composite material. The silicon carbide ceramic product prepared according to this method has silicon carbide as the matrix and a micro-sheet structure as the reinforcing phase. The silicon carbide composite material is densified and has good mechanical properties, which solves the problem of the difficulty of dispersibility of the sheet structure in silicon carbide ceramics and the high densification temperature of the silicon carbide ceramics themselves.

[0022] In addition, the lamellar structure toughened silicon carbide ceramic composite material provided by the present invention has a simple preparation process, good repeatability and strong stability, and is therefore easy to achieve batch production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The microstructure of the hot-pressed sintered SiC ceramic composite material according to Example 1 of the present invention;

[0024] Figure 2 This is the microstructure of the SiC ceramic composite material sintered by spark plasma in Example 2 of the present invention. DETAILED DESCRIPTION

[0025] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is described in detail below in conjunction with specific embodiments. The description in this section is only exemplary and explanatory and should not have any limiting effect on the scope of protection of the present invention.

[0026] The present invention provides a method for preparing a micro-lamellar structure reinforced silicon carbide ceramic composite material, comprising the following steps:

[0027] Silicon carbide powder is used as raw material powder, and micro-lamellar material is used as reinforcement, wherein the micro-lamellar material is graphene sheet and / or silicon carbide whisker; aluminum oxide, yttrium oxide, auxiliary oxide and boron powder are used as sintering aids, wherein the auxiliary oxide is silicon dioxide and / or calcium oxide, and high-pressure sintering below 1760° C. is performed to obtain a micro-lamellar structure reinforced silicon carbide ceramic composite material.

[0028] In view of the problems that lamellar structures are difficult to disperse in silicon carbide ceramics and the high densification temperature of silicon carbide ceramics themselves, the present invention provides a method for preparing a lamellar structure reinforced silicon carbide ceramic composite material, and the prepared silicon carbide ceramic (based) composite material, which has good mechanical properties and high density, and the preparation temperature is relatively low, which is conducive to promotion and application.

[0029] The pressure sintering preparation method of the micro-lamellar structure reinforced silicon carbide ceramic composite material according to a specific embodiment of the present invention comprises the following steps:

[0030] 1) Weigh raw materials, reinforcement and sintering aid powders according to the mass percentage ratio, wherein the micro-sheet material content is 2-8%, the aluminum oxide, yttrium oxide and auxiliary oxide powders account for 5-9wt% in total, and the mass ratio of aluminum oxide, yttrium oxide and auxiliary oxide is 28:49:23; boron powder accounts for 0.5-1wt%, and the balance is silicon carbide powder;

[0031] 2) preparing a dispersion of the micro-lamellar material, preferably adding weighed micro-lamellar material powder into anhydrous ethanol, then adding a silane coupling agent, and ultrasonically dispersing for 2 to 5 hours to obtain a uniformly dispersed dispersion;

[0032] 3) mixing the dispersion of the micro-sheet material with silicon carbide powder, various oxide powders and boron powder, preferably adding a dispersant and performing ball milling;

[0033] 4) drying the ball-milled powder, and then placing it in a pressureless sintering furnace for debinding treatment, wherein the temperature range is preferably set to 400-600° C., and the holding time can be 0.5-2 h;

[0034] 5) The debinding treated silicon carbide ceramic composite material powder is subjected to high pressure sintering at 1700° C. to 1760° C. to prepare a micro-lamellar structure reinforced silicon carbide ceramic composite material.

[0035] The embodiment of the present invention firstly selects submicron-level silicon carbide raw ceramic powder, which can prevent the powder from soft agglomeration during the mixing process and mix uniformly, and the smaller the powder particle size, the higher the surface activity, which helps to promote densification during the sintering process. In the embodiment of the present invention, the silicon carbide powder particle size is 100nm~1μm, preferably 100nm~600nm.

[0036] The embodiment of the present invention improves the strength and fracture toughness of silicon carbide ceramics by introducing a second phase sheet structure, that is, using silicon carbide whiskers or graphene sheets as a reinforcing and toughening phase. Specifically, these materials with micro-sheet structures can be commercially available and added in the form of a dispersion.

[0037] According to the above scheme, the powder type of the micro-sheet material in step 2) is silicon carbide whiskers and / or graphene micro-sheets, and the sheet diameter cross-sectional height can be 0.3-2 μm and the length can be 5-20 μm. The micro-sheet material is treated with a coupling agent, preferably a silane coupling agent; specifically, KBM-602 (N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane) produced by Shin-Etsu Chemical Co., Ltd. of Japan, WD-51 and WD-53 of Hubei Wuda Organic Silicon New Materials Co., Ltd., and A-1120 silane coupling agent (γ-aminoethylaminopropyltrimethoxysilane) of Union Carbide Corporation of the United States are selected. The concentration of the dispersion of the micro-sheet material can be 5-10 mg / ml, and the amount of the coupling agent added is preferably 0.2-0.5% of the volume of the anhydrous ethanol solution. The addition of the silane coupling agent in the preferred embodiment of the present invention can play a good dispersing role on the graphene sheets and silicon carbide whiskers toughened by the micro-sheet structure, and the silane coupling agent can play a bonding role on silicon carbide, promoting the uniform combination of silicon carbide and the micro-sheet structure.

[0038] In an embodiment of the present invention, alumina (aluminum oxide, Al2O3), yttrium oxide (yttrium oxide, Y2O3), auxiliary oxide powder (one or both of calcium oxide CaO and silicon dioxide SiO2), and boron powder are used as sintering aids. Alumina and yttrium oxide mainly play a bonding role; since silicon carbide powder still has excess free carbon during the preparation process, a small amount of boron powder is appropriately added, which can react with the free carbon to generate a trace amount of boron carbide, promoting densification to a certain extent. The embodiment of the present invention reasonably selects the above specific sintering aids, which can produce a liquid phase at a lower temperature, effectively reduce the sintering temperature of sintered silicon carbide ceramics, promote densification, and reduce damage to the lamellar structure.

[0039] In some embodiments, alumina, silica and yttrium oxide are selected, which can form a liquid phase at 1773K. The densification of silicon carbide ceramics can be achieved at only 1750°C through liquid phase sintering, and alumina, yttrium aluminum garnet and γ-SiAlY are formed during the high-temperature cooling process, which has little effect on the high-temperature mechanical properties of the silicon carbide ceramic composite material; and the addition of boron will react with the carbon in the SiC powder and the residual carbon in the dispersant to promote sintering and improve the mechanical properties.

[0040] In addition, the optimal powder particle size of the materials in some embodiments of the present invention is selected as follows: the particle size of boron powder is 1-3 μm, the particle size of each oxide sintering aid powder is 100nm-600nm, preferably 150nm-500nm, and the particle size of silicon carbide powder is 100nm-600nm.

[0041] In the embodiment of the present invention, the silicon carbide and sintering aid powders weighed in step 1) are added to the dispersion of the micro-sheet material in step 2), and the obtained ceramic slurry is ball-milled in a planetary ball mill in the presence of a dispersant, and then can be rotary evaporated and dried for 24 hours to obtain a uniformly dispersed SiC composite powder. According to the above scheme, the preferred planetary ball milling process conditions in step 3) are: the grinding balls are Si3N4 balls, the ball-to-material ratio is 3 to 5:1, the ball milling speed is 100 to 200 rpm / min, and the ball milling time can be 2 to 5 hours, preferably 3 to 4 hours. Among them, the added dispersant is preferably a cationic polymer dispersant, and the German Walker VOK-KD10, VOK-KD2, VOK-KD3 or the British Croda Hypermer KD-1 dispersant can be selected; its added amount accounts for 0.5 to 1.5wt% of the total powder.

[0042] The present invention preferably uses a high-viscosity fiber dispersant, which also acts as a powder stabilizer, and helps to evenly disperse the fiber and powder. The embodiment of the present invention uses a well-bonded sintering aid, which cooperates with a good dispersant to achieve even dispersion and bonding between the lamellar structure and the ceramic powder.

[0043] In the embodiment of the present invention, the powder after ball milling can be placed in a pressureless sintering furnace, preferably at a temperature of 400 to 600°C for debinding treatment, and the powder of the silicon carbide composite material can be obtained by heat preservation. In an embodiment of the present invention, the composite material powder after debinding is subjected to high pressure sintering at 1700°C to 1760°C to obtain a micro-lamellar structure reinforced silicon carbide ceramic composite material. The high pressure sintering can be performed in the form of hot pressing sintering or spark plasma sintering; high pressure combined with the aforementioned pressure sintering process such as the added sintering aid, through high pressure instantaneous liquid phase sintering, the silicon carbide composite material can be densified at a relatively low temperature, while ensuring the good mechanical properties of the material.

[0044] According to the above scheme, the sintering process conditions of step 5) are preferably: under vacuum conditions, firstly, the temperature is raised from room temperature to 1600°C at a heating rate of 10-100°C / min (preferably 15-100°C / min), and then raised to 1700°C-1760°C at 5-15°C / min, and kept warm for 20-60min. During the sintering process, the axial sintering pressure is controlled to be 50-70MPa, preferably 50-60MPa, and finally a dense, microstructure-uniform micro-lamellar structure-reinforced silicon carbide-based ceramic composite material is obtained. In the pressure sintering involved in the embodiment of the present invention, since Al2O3, Y2O3 and SiO2 (CaO) can form a eutectic phase and are in a liquid phase at 1700°C, high-pressure instantaneous liquid phase sintering between 50-70MPa can greatly promote densification and improve mechanical properties.

[0045] The embodiment of the present invention selects a certain high temperature and high pressure sintering system. The high temperature and high pressure instantaneous liquid phase sintering can effectively reduce the sintering temperature and help form a twin structure in silicon carbide ceramics to improve mechanical properties. The preparation process described in the embodiment of the present invention is simple and stable. The above temperature system is also very important. It can avoid excessive residual stress in industrial production and affect the appearance of cracks in the ceramic composite material.

[0046] The present invention provides a micro-lamellar structure reinforced silicon carbide ceramic composite material obtained by the preparation method as described above, which has silicon carbide as a matrix and contains a uniform micro-lamellar structure reinforcement phase, has good mechanical properties such as fracture toughness and flexural strength, and a density of more than 98%; this high-performance silicon carbide-based ceramic product has a wider application prospect.

[0047] The following is a further description of the micro-lamellar structure reinforced silicon carbide ceramic composite material and its pressure sintering preparation method in combination with specific examples. The following materials are commercially available; among them, the particle size of the boron powder is 1 to 3 μm, the purity is 99%, the particle size of each oxide sintering aid powder is 100nm to 600nm, the purity is more than 99%, and the particle size of the silicon carbide powder is 100nm to 600nm, and the purity is 99%. The height of the cross-section of the micro-lamellar material powder is 0.3 to 2 μm, and the length is 5 to 20 μm. The coupling agent is the A-1120 brand silane coupling agent of Union Carbide Corporation of the United States.

[0048] Example 1

[0049] A pressure sintering preparation method for a micro-lamellar structure reinforced silicon carbide ceramic composite material comprises the following steps:

[0050] 1) Weigh raw material powders: 26.85 g silicon carbide powder, 0.588 g aluminum oxide powder, 0.483 g silicon dioxide powder, 1.029 g yttrium oxide powder, 0.9 g graphene powder, and 0.15 g boron powder.

[0051] 2) preparing a graphene microplatelet dispersion: adding 0.9 g of graphene powder to 180 mL of anhydrous ethanol, adding 0.5 mL of a silane coupling agent, and ultrasonically dispersing for 2 h to obtain a uniformly dispersed graphene dispersion;

[0052] 3) Silicon carbide, aluminum oxide, yttrium oxide, boron powder and silicon dioxide are added to the prepared graphene dispersion, and the obtained ceramic slurry is ball-milled, and 0.3 g of Hypermer KD-1 dispersant is added at the same time. The ball milling process is: Si3N4 grinding balls are selected, the ball-to-material ratio is 3:1, the rotation speed is 150rpm / min, the ball milling time is 3h, and after rotary evaporation and drying, a uniformly dispersed SiC composite powder is obtained.

[0053] 4) The ball-milled and dried powder is placed in a pressureless sintering furnace and subjected to a binder removal treatment at 400° C. to obtain a powder of the silicon carbide composite material.

[0054] 5) placing the mixed powder after debinding in step 4) in a graphite mold, and performing hot pressing sintering in a hot pressing furnace. Under vacuum conditions, the temperature is first increased from room temperature to 1600° C. at a heating rate of 15° C. / min, and then increased to 1730° C. at a heating rate of 10° C. / min, and kept warm for 40 minutes. During the sintering process, the axial sintering pressure is controlled to be 60 MPa to obtain a dense silicon carbide ceramic composite material with uniform microstructure.

[0055] Example 2

[0056] A pressure sintering preparation method for a micro-lamellar structure reinforced silicon carbide ceramic composite material comprises the following steps:

[0057] 1) Weigh raw materials and other powders: 26.4g silicon carbide powder, 0.672g aluminum oxide powder, 0.552g silicon dioxide powder, 1.176g yttrium oxide powder, 1.5g silicon carbide whiskers, and 0.2g boron powder.

[0058] 2) preparing a micro-lamellar material dispersion: adding 1.5 g of silicon carbide whiskers to 300 mL of alcohol, adding 1.2 mL of a silane coupling agent, and ultrasonically dispersing for 3 h to obtain a uniformly dispersed silicon carbide whisker dispersion;

[0059] 3) The powder of step 1) and the dispersion of step 2) were mixed in a planetary ball mill, and 0.2 g of VOK-KD2 dispersant was added. The ball milling process was as follows: Si3N4 grinding balls were selected, the ball-to-material ratio was 4:1, the ball milling speed was 100 rpm / min, the ball milling time was 4 h, and then rotary evaporation was performed for 24 h to obtain a uniformly dispersed SiC composite powder.

[0060] 4) The ball-milled and dried powder is placed in a pressureless sintering furnace and subjected to a binder removal treatment at 400° C. to obtain a powder of the silicon carbide composite material.

[0061] 5) placing the mixed powder after debinding in step 4) in a graphite mold and performing spark plasma sintering. Under vacuum conditions, the temperature is first increased from room temperature to 1600°C at a heating rate of 100°C / min, and then increased to 1750°C at a heating rate of 10°C / min, and kept warm for 40 minutes. During the sintering process, the axial sintering pressure is controlled to be 55 MPa to obtain a dense, microstructured, uniformly reinforced micro-lamellar structure silicon carbide ceramic composite ceramic.

[0062] Example 3

[0063] A pressure sintering preparation method for a micro-lamellar structure reinforced silicon carbide ceramic composite material comprises the following steps:

[0064] 1) Weigh raw materials and other powders: 236.25g silicon carbide powder, 6.048g aluminum oxide powder, 4.968g silicon dioxide powder, 10.584g yttrium oxide powder, 10.8g silicon carbide whiskers, and 1.38g boron powder.

[0065] 2) preparing a micro-lamellar material dispersion: adding 10.8 g of silicon carbide whiskers to 1500 mL of alcohol, adding 6 mL of a silane coupling agent, and ultrasonically dispersing for 5 h to obtain a uniformly dispersed silicon carbide whisker dispersion;

[0066] 3) Mix the powder of step 1) and the dispersion of step 2) in a planetary ball mill, and add 2g of VOK-KD2 slurry dispersant. The ball milling process is: use Si3N4 grinding balls, the ball-to-material ratio is 3:1, the ball milling speed is 100rpm / min, the ball milling time is 4h, and the mixed powder after ball milling is dried to obtain a uniformly dispersed SiC composite powder;

[0067] 4) The dried powder is placed in a pressureless sintering furnace, subjected to a binder removal treatment at 500° C., and kept warm for 1 hour to obtain a powder of the silicon carbide composite material.

[0068] 5) placing the mixed powder after debinding in step 4) in a graphite mold, and performing hot pressing sintering in a hot pressing furnace. Under vacuum conditions, the temperature is first increased from room temperature to 1600°C at a heating rate of 15°C / min, and then increased to 1760°C at a heating rate of 10°C / min, and kept warm for 1 hour. During the sintering process, the axial sintering pressure is controlled to be 50 MPa to obtain a dense silicon carbide ceramic composite material with uniform microstructure.

[0069] The performance of the obtained silicon carbide ceramic composite material was tested according to the methods of GBT 23806-2009 and GB T 6569-2006 in the art, and the results are as follows. In Table 1, the fracture toughness of the reinforced SiC composite ceramic prepared in the embodiment of the present invention is 6.1 MPa·m 0.5 The above, the bending strength is higher than 600MPa (much higher than the general silicon carbide ceramic material), the density can reach more than 98%, with good mechanical strength and density. Figure 1 The microstructure of the hot-pressed sintered SiC ceramic composite material of Example 1; Figure 2 The microstructure of the SiC ceramic composite material sintered by spark plasma sintering in Example 2. The toughened lamellar microstructure can be seen in the figure, and it is evenly distributed in the silicon carbide matrix structure.

[0070] Table 1 Mechanical properties of samples in the examples

[0071]

[0072] Finally, it should be noted that the specific embodiments described in this article are merely examples of the spirit of the present invention, and are not intended to limit the implementation methods of the present invention. Those skilled in the art of the present invention may make other modifications or additions to the described embodiments and replace them in a similar manner. It is not necessary and impossible to provide all the implementation methods here. These obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A method for preparing a micro-lamellar structure reinforced silicon carbide ceramic composite material, It is characterized in that The following steps are involved: Silicon carbide powder is used as raw material powder, and micro-sheet material is used as reinforcement, wherein the micro-sheet material is graphene sheet and / or silicon carbide whisker; aluminum oxide, yttrium oxide, auxiliary oxide and boron powder are used as sintering aids, wherein the auxiliary oxide is silicon dioxide and / or calcium oxide, and the specific steps are: mixing the dispersion of the micro-sheet material with the silicon carbide powder and the sintering aid, and ball milling; the micro-sheet material has a sheet diameter cross-sectional height of 0.2 to 2 μm and a length of 5 to 20 μm; in the mixed material, the micro-sheet material content is 2 to 8 wt%, the aluminum oxide, yttrium oxide and auxiliary oxide powders account for a total of 5 to 9 wt%, the boron powder accounts for 0.5 to 1 wt%, and the balance is silicon carbide powder; The ball-milled powder is subjected to a binder removal treatment to obtain a composite material powder; and a micro-lamellar structure-reinforced silicon carbide ceramic composite material is obtained by high-pressure sintering at 1700-1760°C.

2. The preparation method according to claim 1, It is characterized in that The particle size of the silicon carbide powder is 100nm-1μm.

3. The preparation method according to claim 1, It is characterized in that The micro-sheet material is treated with a silane coupling agent.

4. The preparation method according to any one of claims 1 to 3, It is characterized in that The particle size of the boron powder is 1-3 μm, and the particle sizes of the aluminum oxide, yttrium oxide and auxiliary oxide powders are all 100 nm-800 nm.

5. The preparation method according to any one of claims 1 to 3, It is characterized in that The ball milling is planetary ball milling and is carried out in the presence of a dispersant; the amount of the dispersant used accounts for 0.5-1.5wt% of the total amount of the powder.

6. The preparation method according to claim 5, It is characterized in that The planetary ball mill is made of Si 3 N 4 Grinding balls, ball-to-material ratio is 3-5:1, and the ball mill speed is 100-300rpm.

7. The preparation method according to any one of claims 1 to 3, It is characterized in that The high-pressure sintering is carried out under vacuum conditions, firstly heating from room temperature to 1600°C at a heating rate of 10-100°C / min, then heating to 1700°C-1760°C at a heating rate of 5-15°C / min, and keeping the temperature for 20-60 minutes. During the sintering process, the axial sintering pressure is controlled to be 50-70MPa.

8. The micro-lamellar structure reinforced silicon carbide ceramic composite material obtained by the preparation method according to any one of claims 1 to 7 has a density of more than 98%.