A water-resistant bonding spray-coated quick-setting liquid rubber waterproof composite coating and its preparation method and application

By combining modified emulsified asphalt and latex, the water absorption rate of sprayed fast-gel rubber asphalt waterproof coating film is reduced, and the problem of decreasing adhesion force of the waterproof coating film in an immersion environment is solved, thereby achieving higher water resistance.

CN116622289BActive Publication Date: 2024-11-26STATE GRID XINYUAN GRP CO LTD +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310402703.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-14
Publication Date
2024-11-26
Estimated Expiration
2043-04-14

AI Technical Summary

Technical Problem

Sprayed fast-coagulation rubber asphalt waterproof coating film in immersion environments such as water conservancy reservoirs, pumped storage power stations, etc., the increase in water absorption rate leads to a decrease in the adhesion between the waterproof coating film and concrete.

Method used

Use water-resistant bonded spray-coagulation liquid rubber waterproof composite coating, consisting of modified emulsified asphalt, polymer emulsion, tackifying resin, filler, defoaming agent and thickening agent. By combining modified emulsified asphalt and latex, it reduces the Water absorption and enhance bonding properties.

Benefits of technology

It significantly reduces the water absorption rate of the composite coating film, improves the adhesion to the surface of the base layer, and enhances the waterproof performance in the immersion environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116622289B_ABST
    Figure CN116622289B_ABST
Patent Text Reader

Abstract

The present application provides a water-resistant adhesive spray quick-setting liquid rubber waterproof composite coating and a preparation method and application thereof, and specifically relates to the technical field of chemical materials. The water-resistant adhesive spray quick-setting liquid rubber waterproof composite coating consists of a first coating and a second coating; wherein, based on 100 parts by weight, the first coating is composed of 30-60 parts of modified emulsified asphalt, 30-60 parts of polymer emulsion, 3-10 parts of tackifying resin, 5-30 parts of filler, 0.5-2.0 parts of defoaming agent and 0.5-3.0 parts of thickener; the second coating is composed of 20-70 parts of modified emulsified asphalt, 30-70 parts of latex, 10-50 parts of slurry, 0.5-2.0 parts of defoaming agent, 0.5-3.0 parts of stabilizer, 0.5-2.0 parts of UV-resistant additive, 1-3 parts of coupling agent and 1-3 parts of film-forming additive. The water-resistant bonding spray-coated quick-setting liquid rubber waterproof composite coating proposed in the present application reduces the water absorption rate of the composite coating, improves the water-resistant bonding performance of the composite coating, and can be used for base surfaces in immersion environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of chemical materials, and in particular to a water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating, and a preparation method and application thereof. Background Art

[0002] Spraying quick-setting rubber asphalt waterproofing materials are widely used in building waterproofing, high-speed rail and subway, etc. However, in soaking environments such as water conservancy reservoirs and pumped storage power stations, the spraying quick-setting rubber asphalt waterproofing membrane has an increased water absorption rate after a long period of soaking, which reduces the bonding strength between the waterproofing membrane and the concrete.

[0003] Therefore, in the field of spray quick-setting waterproof coatings, it is necessary to develop a water-resistant adhesive rubber asphalt waterproof coating with low water absorption and good bonding performance. Summary of the invention

[0004] The present invention provides a water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating and a preparation method and application thereof, so as to solve the problem that the water absorption rate of the rubber asphalt waterproof coating increases, resulting in a decrease in the adhesion between the waterproof coating and the base surface in an immersion environment.

[0005] To solve the above problems, in a first aspect, the present invention provides a water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating, wherein the water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating is composed of a first coating and a second coating;

[0006] Wherein, based on 100 parts by weight, the first coating is mixed with 30-60 parts of modified emulsified asphalt, 30-60 parts of polymer emulsion, 3-10 parts of tackifying resin, 5-30 parts of filler, 0.5-2.0 parts of defoaming agent and 0.5-3.0 parts of thickener;

[0007] Based on 100 parts by weight, the second coating is mixed with 20-70 parts of modified emulsified asphalt, 30-70 parts of latex, 10-50 parts of slurry, 0.5-2.0 parts of defoaming agent, 0.5-3.0 parts of stabilizer, 0.5-2.0 parts of UV resistant additive, 1-3 parts of coupling agent and 1-3 parts of film-forming additive.

[0008] Preferably, the modified emulsified asphalt is obtained by reacting 50-70 parts of the first modified asphalt and 0.5-3.0 parts of an emulsifier;

[0009] The first modified asphalt is obtained by reacting 50-70 parts of base asphalt, 5-10 parts of filler oil and 1-3 parts of modifier;

[0010] Preferably, the emulsifier is an anionic emulsifier or a nonionic emulsifier;

[0011] Preferably, the filler oil is at least one of naphthenic oil and aromatic oil;

[0012] Preferably, the modifier is at least one of styrene-butadiene rubber and SBS rubber.

[0013] Preferably, the polymer emulsion is at least one of styrene-butadiene rubber latex, chloroprene rubber latex, pressure-sensitive adhesive latex, acrylic emulsion, polyurethane emulsion, and epoxy emulsion;

[0014] Preferably, the tackifying resin is at least one of coumarone resin, terpene resin, rosin resin and petroleum resin;

[0015] Preferably, the filler is at least one of calcium carbonate, barium sulfate, titanium dioxide, and silicon powder;

[0016] Preferably, the defoaming agent is a silicone defoaming agent;

[0017] Preferably, the thickener is at least one of a cellulose thickener and a water-soluble acrylic thickener.

[0018] Preferably, the slurry is mixed with 3-6 parts of dispersant, 20-70 parts of deionized water, 1-3 parts of fumed silica, 20-70 parts of filler and 0.2-3.0 parts of defoamer;

[0019] Preferably, the dispersant is a polymer dispersant;

[0020] Preferably, the fumed silica is hydrophilic fumed silica;

[0021] Preferably, the filler is at least one of calcium bicarbonate, calcium carbonate, barium sulfate, titanium dioxide, and silicon powder;

[0022] Preferably, the defoaming agent is a silicone defoaming agent.

[0023] Preferably, the latex is at least one of chloroprene rubber latex, styrene-butadiene rubber latex, natural latex, acrylic latex, nitrile latex, and butyl latex;

[0024] Preferably, the defoaming agent is a silicone defoaming agent;

[0025] Preferably, the stabilizer is at least one of a vinyl silane coupling agent and calcium sulfate;

[0026] Preferably, the UV-resistant additive is at least one of the aminophenol antioxidants 1010, salicylates, and benzophenones;

[0027] Preferably, the coupling agent is at least one of a titanate coupling agent, a silane coupling agent, and an aluminate coupling agent;

[0028] Preferably, the film-forming aid is at least one of alcohol ester dodecanedione, propylene glycol butyl ether, and ethylene glycol.

[0029] Preferably, the first coating is a mixture of 30-35 parts of modified emulsified asphalt, 30 parts of polymer emulsion, 5-10 parts of tackifying resin, 25 parts of filler, 2 parts of defoamer and 3 parts of thickener;

[0030] Preferably, the second coating is a mixture of 25-55 parts of modified emulsified asphalt, 30-60 parts of latex, 10-15 parts of slurry, 0.3-0.5 parts of defoamer, 0.5-3.0 parts of stabilizer, 1.5-1.7 parts of UV resistant additive, 1.5-2.0 parts of coupling agent and 1.0-1.5 parts of film-forming additive.

[0031] Preferably, the first coating is a mixture of 30 parts of modified emulsified asphalt, 30 parts of polymer emulsion, 10 parts of tackifying resin, 25 parts of filler, 2 parts of defoamer and 3 parts of thickener;

[0032] Preferably, the second coating is a mixture of 25 parts of modified emulsified asphalt, 55 parts of latex, 15 parts of slurry, 0.4 parts of defoamer, 0.6 parts of stabilizer, 1.6 parts of UV resistant additive, 2.0 parts of coupling agent and 1.0 parts of film-forming additive.

[0033] In a second aspect, the present invention provides a method for preparing the water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating as described in the first aspect, comprising:

[0034] S1, preparing a first coating, comprising:

[0035] S11, heating the base asphalt to 140-160° C., stirring for 10-20 minutes, adding the filler oil and the modifier, further heating to 160-180° C., stirring for more than 4 hours, to obtain the first modified asphalt;

[0036] S12, mixing the emulsifier soap solution with the first modified asphalt, and then emulsifying the mixture by high-speed shearing in a colloid mill to obtain the modified emulsified asphalt;

[0037] S13, mixing 30-60 parts of the modified emulsified asphalt with 30-60 parts of a polymer emulsion, 3-10 parts of a tackifying resin, 5-30 parts of a filler, 0.5-2.0 parts of a defoaming agent and 0.5-3.0 parts of a thickener according to a certain proportion and stirring for 30 minutes to obtain the first coating;

[0038] S2, preparing a second coating, comprising:

[0039] S21, adding a dispersant, fumed silica, a filler and a defoamer into deionized water, stirring evenly, and grinding and dispersing with a grinder to obtain the slurry;

[0040] S22, 10-50 parts of the slurry, 20-70 parts of the modified emulsified asphalt, 30-70 parts of latex, 0.5-2.0 parts of defoaming agent, 0.5-3.0 parts of stabilizer, 0.5-2.0 parts of UV resistant additive, 1-3 parts of coupling agent and 1-3 parts of film-forming additive are mixed and stirred in proportion for 30 minutes to obtain the second coating.

[0041] In a third aspect, the present invention provides an application of a water-resistant adhesive spray-applied quick-setting liquid rubber waterproof composite coating, wherein a first coating is applied to the surface of a base layer to form a first coating film, and a second coating is applied to the surface of the first coating film to form a second coating film.

[0042] Preferably, the thickness of the first coating film is 0.1-0.4 mm, and the thickness of the second coating film is 1.5-2.5 mm.

[0043] The present invention provides a water-resistant bonding spray quick-setting liquid rubber waterproof composite coating and a preparation method and application thereof. Compared with the prior art, the present application has the following advantages:

[0044] (1) The water-resistant bonding spray-coated quick-setting liquid rubber waterproof composite coating of the present invention uses an acrylic emulsion that can be demulsified and has a low water absorption rate in the composite coating, so that the formed composite coating film is more compact and has a lower water absorption rate, thereby enhancing the water-resistant bonding performance of the composite coating film;

[0045] (2) In the water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating of the present invention, the addition of inorganic hydrophobic filler reduces the water absorption rate of the composite coating film, and the inorganic hydrophobic filler and the non-polar long chain of latex reasonably block the contact between the composite coating film and water, significantly reducing the water absorption rate of the composite coating film and enhancing the water-resistant bonding performance of the composite coating film;

[0046] (3) The water-resistant adhesive spray-applied quick-setting liquid rubber waterproof composite coating of the present invention, the first coating and the second coating are both prepared by modified emulsified asphalt, the first coating and the second coating are applied to the surface of the base layer in sequence to form a compatible composite coating film. Since the first coating seals part of the dust in the base layer, the treatment requirements for the surface of the base layer are reduced, and the addition of the tackifying resin further enhances the bonding force between the composite coating film and the surface of the base layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 The present invention is a flowchart of the steps of a method for preparing a water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating according to an embodiment of the present invention. DETAILED DESCRIPTION

[0048] In order to make the above-mentioned purposes, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. The embodiments of the present invention are described in detail below. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0049] The invention provides a water-resistant adhesive spray quick-setting liquid rubber waterproof composite coating and a preparation method and application thereof. The prepared water-resistant adhesive spray quick-setting liquid rubber waterproof composite coating has low water absorption and excellent bonding performance.

[0050] The invention provides a water-resistant bonding spray quick-setting liquid rubber waterproof composite coating, which consists of a first coating and a second coating. Based on 100 parts by weight, the first coating is formed by mixing 30-60 parts of modified emulsified asphalt, 30-60 parts of polymer emulsion, 3-10 parts of tackifying resin, 5-30 parts of filler, 0.5-2.0 parts of defoamer and 0.5-3.0 parts of thickener; the second coating is formed by mixing 20-70 parts of modified emulsified asphalt, 30-70 parts of latex, 10-50 parts of slurry, 0.5-2.0 parts of defoamer, 0.5-3.0 parts of stabilizer, 0.5-2.0 parts of UV-resistant additive, 1-3 parts of coupling agent and 1-3 parts of film-forming additive.

[0051] Among them, the water-resistant adhesive spray quick-setting liquid rubber waterproof composite coating provided by the present invention is composed of a first coating and a second coating, the first coating is a mixture of modified emulsified asphalt, polymer emulsion, tackifying resin, filler, defoaming agent and thickener, and the second coating is a mixture of modified emulsified asphalt, latex, hydrophilic slurry, defoaming agent, stabilizer, UV-resistant additive coupling agent and film-forming additive. The modified emulsified asphalt has high stability and low water absorption. After the modified emulsified asphalt, polymer emulsion and filler in the first coating are mixed, the compatibility of the mixed system in the first coating can be improved, so that the stability and adhesion of the first coating are improved; the addition of the tackifying resin improves the adhesion between the first coating and the surface of the base layer, and after the first coating is quickly cured into a film, it is firmly bonded to the surface of the base layer; further, the filler in the first coating is preferably an inorganic hydrophobic filler, because the non-polar long chain on the surface of the inorganic hydrophobic filler blocks the contact between the first coating and water, significantly reducing the water absorption of the first coating; wherein, the defoaming agent can eliminate factors such as bubbling and bubbles generated during the preparation process that affect the performance of the first coating; wherein, the thickener can enable the first coating to have good thixotropy, good storage stability and workability. The second coating mainly adopts modified emulsified asphalt with low water absorption and latex with low water absorption as the base material, which reduces the water absorption of the second coating; the slurry prepared by gas-phase silica with improved storage stability and dispersibility of powdered products further reduces the water absorption of the second coating; among them, the defoaming agent can eliminate factors affecting the performance of the second coating such as bubbling and bubbles generated in the preparation process; the stabilizer is beneficial to the long-term storage stability of the second coating; the UV-resistant additive can extend the service life of the second coating; at the same time, the addition of coupling agent and film-forming agent in the second coating enhances the strength and density of the second coating.

[0052] Preferably, in the embodiment of the present application, the first coating can be mixed by 30-35 parts of modified emulsified asphalt, 30 parts of polymer emulsion, 5-10 parts of tackifying resin, 25 parts of filler, 2 parts of defoaming agent and 3 parts of thickener;

[0053] For example, the modified emulsified asphalt component in the first coating may be 30 parts, 31 parts, 32 parts, 33 parts, 34 parts, 35 parts, etc.; the tackifying resin component may be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, etc. Those skilled in the art may set it according to the needs, and the embodiments of the present application will not be described in detail.

[0054] Preferably, in an embodiment of the present application, the second coating is a mixture of 25-55 parts of modified emulsified asphalt, 30-60 parts of latex, 10-15 parts of slurry, 0.3-0.5 parts of defoaming agent, 0.5-3.0 parts of stabilizer, 1.5-1.7 parts of UV resistant additive, 1.5-2.0 parts of coupling agent and 1.0-1.5 parts of film-forming additive.

[0055] For example, the modified emulsified asphalt in the second coating may contain 25 parts, 30 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, etc.; the latex may contain 30 parts, 35 parts, 35 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, etc.; the slurry may contain 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, etc.; the defoamer may contain 0.3 parts, 0.4 parts, 0.5 parts, etc. ; The component of the stabilizer can be 0.5 parts, 1.0 parts, 1.5 parts, 2.0 parts, 2.5 parts, 3.0 parts, etc.; The component of the UV-resistant additive can be 1.5 parts, 1.6 parts, 1.7 parts, etc.; The component of the coupling agent can be 1.5 parts, 1.6 parts, 1.7 parts, 1.8 parts, 1.9 parts, 2.0 parts, etc.; The component of the film-forming additive can be 1.0 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, etc. Those skilled in the art can make settings according to needs, and the embodiments of this application will not be repeated in detail.

[0056] In the embodiment of the present invention, the modified emulsified asphalt is obtained by reacting 50-70 parts of the first modified asphalt and 0.5-3.0 parts of the emulsifier; wherein the first modified asphalt is obtained by reacting 50-70 parts of the base asphalt, 5-10 parts of the filler oil and 1-3 parts of the modifier. The base asphalt is modified by adding the filler oil and the modifier, and the modified emulsified asphalt modified by the filler oil and the modifier has high stability and increases the compatibility of the asphalt with the polymer emulsion and the filler; the addition of the filler oil increases the carbon-hydrogen ratio of the modified emulsified asphalt and reduces the water absorption rate of the modified emulsified asphalt; the addition of the modifier makes the surface of the coating formed after the modified emulsified asphalt is mixed with the latex more dense, and it is more difficult for water to penetrate, which significantly reduces the water absorption rate of the first coating and the second coating. In the embodiment of the present invention, the filler oil in the modified emulsified asphalt is at least one of cycloparaffinic oil and aromatic oil. The filler oil can increase the carbon-hydrogen ratio of the modified emulsified asphalt and reduce the water absorption rate, thereby reducing the water absorption rate of the first coating and the second coating. In the embodiment of the present invention, the modifier in the modified emulsified asphalt is at least one of styrene-butadiene rubber and SBS rubber. The modifier in this embodiment is preferably a polymer. This is because after the modified emulsified asphalt modified by the polymer modifier is mixed with latex, the coating surface formed is denser and water is more difficult to penetrate, which significantly reduces the water absorption rate of the first coating and the second coating.

[0057] In the embodiments of the present application, the emulsifier is an anionic emulsifier or a nonionic emulsifier. In the embodiments of the present application, the emulsifier is preferably at least one of rosin and its derivatives, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene ether, and octylphenol polyoxyethylene ether. In the embodiments of the present invention, the emulsified asphalt is preferably anionic emulsified asphalt. This is because in the emulsified asphalt solution, due to the different emulsifiers used, the asphalt particles will carry (+) (-) charges. For nonionic emulsified asphalt, the emulsifier in the emulsion is not ionized in water, but has hydrophilic and lipophilic groups, has strong emulsifying ability, and has a stronger dispersing effect on rubber latex, so that a more uniformly dispersed emulsion system can be obtained. For anionic emulsified asphalt, the H + The lower the content of ions, the less likely it is that H + The ions combine with free radicals in the curing process of the water-resistant adhesive spray quick-setting liquid rubber waterproof composite coating to reduce the free radical content, thereby avoiding inhibiting the curing reaction of the water-resistant adhesive spray quick-setting liquid rubber waterproof composite coating. Based on the improvement of the bonding resistance of the first coating, in the embodiment of the present application, the modified emulsified asphalt is selected as the base material of the first coating. This is because the modified emulsified asphalt can improve the performance of the first coating together with the latex, so that the first coating formed by the first coating can be more compact, and the water absorption rate of the first coating is significantly reduced. In the embodiment of the present application, the polymer emulsion is at least one of styrene-butadiene rubber latex, chloroprene rubber latex, pressure-sensitive adhesive latex, acrylic emulsion, polyurethane emulsion, and epoxy emulsion; wherein, since the polymer emulsion is the main base material of the first coating, thus, in the embodiment of the present application, an acrylic emulsion that can be demulsified and has low water absorption and at least one of styrene-butadiene rubber, chloroprene rubber, pressure-sensitive adhesive latex, polyurethane emulsion, and epoxy emulsion with low water absorption are selected as the polymer emulsion to achieve the purpose of reducing the water absorption rate of the first coating.

[0058] In the embodiment of the present application, the tackifying resin is at least one of coumarone resin, terpene resin, rosin resin, and petroleum resin, and the role of the tackifying resin is to improve the bonding force between the first coating and the surface of the base layer; during use, due to the addition of the tackifying resin that can enhance the bonding force, the bonding force between the first coating and the surface of the base layer can be improved. In the embodiment of the present application, the filler of the first coating is at least one of calcium carbonate, barium sulfate, titanium dioxide, and silicon micropowder. The filler in the embodiment of the present application is preferably an inorganic hydrophobic filler, because the non-polar long chain of the inorganic hydrophobic filler can block contact with water, can block contact between the first coating and water, reduce the water absorption rate of the first coating, and improve the bonding force between the first coating and the surface of the base layer; during use, due to the addition of the inorganic hydrophobic filler that can block contact with water, can block contact between the first coating and water, and improve the bonding resistance of the first coating.

[0059] In the embodiment of the present application, the defoaming agent is an organosilicon defoaming agent; wherein, since bubbles and bulges generated during the preparation of the rubber asphalt waterproof coating will affect the performance of the rubber asphalt waterproof coating, the defoaming agent is added to the first coating to eliminate the bubbles and bulges generated during the preparation of the rubber asphalt waterproof coating, which are factors that affect the performance of the rubber asphalt waterproof coating. In the embodiment of the present application, the present application preferably uses an organosilicon defoaming agent, because the organosilicon defoaming agent has excellent stability, reinforcement, thickening and thixotropy.

[0060] In the embodiment of the present application, the thickener is at least one of a cellulose thickener and a water-soluble acrylic thickener; wherein, since the thickener is added to the first coating, the fluid properties of the first coating system can be effectively changed to make it thixotropic, thereby giving the first coating good storage stability and workability. Adding the thickener to the first coating can enable the first coating to have good thixotropy, good storage stability and workability; in the embodiment of the present application, a cellulose thickener is preferably used as the thickener in the first coating, because the hydrophobic main chain of the cellulose thickener molecule associates with the surrounding water molecules through hydrogen bonds, thereby increasing the fluid volume of the polymer itself and reducing the space for free activity of the particles, thereby increasing the system viscosity of the first coating.

[0061] Preferably, in the embodiment of the present application, the first coating can be mixed by 30 parts of modified emulsified asphalt, 30 parts of polymer emulsion, 10 parts of tackifying resin, 25 parts of filler, 2 parts of defoaming agent and 3 parts of thickener;

[0062] As an example, in the embodiment of the present application, the first coating may be a mixture of 30 parts of modified emulsified asphalt, 30 parts of acrylic emulsion, 10 parts of coumarone resin, 25 parts of calcium carbonate, 2 parts of silicone defoamer and 3 parts of cellulose thickener;

[0063] The first coating may be a mixture of 30 parts of modified emulsified asphalt, 30 parts of styrene-butadiene rubber latex, 10 parts of terpene resin, 25 parts of barium sulfate, 2 parts of silicone defoamer and 3 parts of water-soluble acrylic thickener;

[0064] The first coating may be a mixture of 30 parts of modified emulsified asphalt, 30 parts of chloroprene rubber latex, 10 parts of rosin resin, 25 parts of titanium dioxide, 2 parts of silicone defoamer and 3 parts of cellulose thickener;

[0065] The first coating may be a mixture of 30 parts of modified emulsified asphalt, 30 parts of pressure-sensitive adhesive latex, 10 parts of petroleum resin, 25 parts of silicon powder, 2 parts of organosilicon defoamer and 3 parts of water-soluble acrylic thickener;

[0066] The first coating may be a mixture of 30 parts of modified emulsified asphalt, 30 parts of polyurethane emulsion, 10 parts of coumarone resin, 25 parts of calcium carbonate, 2 parts of silicone defoamer and 3 parts of cellulose thickener;

[0067] The first coating may be a mixture of 30 parts of modified emulsified asphalt, 30 parts of epoxy emulsion, 10 parts of coumarone resin, 25 parts of calcium carbonate, 2 parts of silicone defoamer and 3 parts of cellulose thickener;

[0068] Those skilled in the art can make settings according to requirements, and the embodiments of the present application will not be described in detail.

[0069] In the embodiment of the present application, the slurry is mixed with 3-6 parts of dispersant, 20-70 parts of deionized water, 1-3 parts of fumed silica, 20-70 parts of filler and 0.2-3.0 parts of defoamer. In the present embodiment, the dispersant is a polymer dispersant. BYK190 and BYK192 are preferably used as dispersants in the embodiment of the present application. The dispersant is conducive to the dispersion of each component in the slurry in the slurry mixing system. In the embodiment of the present application, the fumed silica is preferably hydrophilic fumed silica, because the hydrophilic fumed silica has a good anti-settling effect, which prevents the deposition of each component in the slurry mixing system and affects the performance of the second coating. In the embodiment of the present application, the filler is preferably an inorganic hydrophobic filler, because the non-polar long chain of the inorganic hydrophobic filler can block contact with water, so that the prepared coating can block contact with water, wherein the filler of the slurry is preferably at least one of calcium bicarbonate, calcium carbonate, barium sulfate, titanium dioxide, and silicon powder. In the embodiment of the present application, the defoaming agent is a silicone defoaming agent, and BYK-018, BYK-022, and BYK-024 are preferably used as the defoaming agent in the embodiment of the present application.

[0070] Based on the case of reducing the water absorption rate of the second coating, in the embodiment of the present application, modified emulsified asphalt is selected as the substrate of the second coating, because the modified emulsified asphalt can improve the performance of the second coating together with latex, so that the formed second coating film can be more compact, and the water absorption rate of the second coating film is significantly reduced. In the embodiment of the present application, the latex is at least one of chloroprene rubber latex, styrene butadiene rubber latex, natural latex, acrylic latex, nitrile latex, and butyl latex; because it is necessary to reduce the water absorption rate of the second coating, in the embodiment of the present application, the latex is selected to be at least one of chloroprene rubber latex, styrene butadiene rubber latex, natural latex, acrylic latex, nitrile latex, and butyl latex with low water absorption rate; in the embodiment of the present application, acrylic latex with demulsifiable and low water absorption rate is preferably used as latex, because acrylic emulsion has excellent antioxidant and anti-ultraviolet aging properties, and has high bonding strength and good water resistance.

[0071] In the embodiment of the present application, the slurry can further reduce the water absorption rate of the second coating, because the slurry in the embodiment of the present application adds an inorganic hydrophobic filler, and the inorganic hydrophobic filler and the non-polar long chain of the latex block the contact between the second coating and water. In the embodiment of the present application, the defoamer is an organosilicon defoamer. In the embodiment of the present application, BYK-018, BYK-022, and BYK-024 are preferably used as defoamers, because the defoamer can eliminate the factors that affect the performance of the waterproof coating, such as bubbles and bulges generated during the preparation process of the rubber asphalt waterproof coating; in the embodiment of the present application, the stabilizer is at least one of a vinyl silane coupling agent and calcium sulfate, and the stabilizer is conducive to the stability of the second coating during long-term storage.

[0072] In the embodiments of the present application, the UV-resistant additive is at least one of the hydroxylated phenol antioxidants 1010, salicylates, and benzophenones; preferably, the UV-resistant additive in the embodiments of the present application is the hydroxylated phenol antioxidant 1010; wherein, since the rubber asphalt waterproof coating is easily affected by ultraviolet rays, the aging of the coating is accelerated and its service life is shortened, a UV-resistant additive is added to the second coating to extend the service life of the second coating.

[0073] In the embodiments of the present application, the coupling agent is at least one of a titanate coupling agent, a silane coupling agent, and an aluminate coupling agent; in the embodiments of the present application, the coupling agent is preferably a silane coupling agent; wherein the silane coupling agent can improve the bonding strength of the second coating, because the silane coupling agent has two functional groups with different chemical properties in its molecules: one group can be combined with the bonded base material; and the other group can be combined with the polymer material or the adhesive, thereby forming a strong chemical bond at the bonding interface, effectively improving the bonding strength.

[0074] In the embodiments of the present application, the film-forming aid is at least one of alcohol ester twelve, propylene glycol butyl ether, and ethylene glycol; in the embodiments of the present application, the preferred film-forming aid is alcohol ester twelve; wherein the film-forming aid can promote the plastic flow and elastic deformation of the polymer compound, improve the coagulation performance of the second coating, and effectively improve the film-forming performance of the second coating; the coupling agent and film-forming aid added to the second coating of the present application can enhance the strength and density of the modified emulsified asphalt, and at the same time can also enhance the density of the latex, thereby enhancing the strength and density of the second coating film made of the second coating.

[0075] Preferably, in an embodiment of the present application, the second coating can be mixed by 25 parts of modified emulsified asphalt, 55 parts of latex, 15 parts of slurry, 0.4 parts of defoaming agent, 0.6 parts of stabilizer, 1.6 parts of UV resistant additive, 2.0 parts of coupling agent and 1.0 parts of film-forming additive.

[0076] As an example, in the embodiment of the present application, the second coating can be mixed with 25 parts of modified anionic emulsified asphalt, 55 parts of acrylic emulsion, 15 parts of slurry, 0.4 parts of silicone defoamer, 0.6 parts of calcium sulfate, 1.6 parts of hindered aminophenol antioxidant 1010, 2.0 parts of silane coupling agent and 1.0 parts of alcohol ester dodecahydrate;

[0077] The second coating may be mixed with 25 parts of modified anionic emulsified asphalt, 55 parts of chloroprene rubber latex, 15 parts of slurry, 0.4 parts of silicone defoamer, 0.6 parts of vinyl silane coupling agent, 1.6 parts of salicylate, 2.0 parts of titanate coupling agent and 1.0 parts of propylene glycol butyl ether;

[0078] The second coating may be mixed with 25 parts of modified anionic emulsified asphalt, 55 parts of styrene-butadiene rubber latex, 15 parts of slurry, 0.4 parts of silicone defoamer, 0.6 parts of calcium sulfate, 1.6 parts of benzophenone, 2.0 parts of aluminate coupling agent and 1.0 parts of ethylene glycol;

[0079] The second coating can be mixed with 25 parts of modified anionic emulsified asphalt, 55 parts of natural latex, 15 parts of slurry, 0.4 parts of silicone defoamer, 0.6 parts of calcium sulfate, 1.6 parts of hindered aminophenol antioxidant 1010, 2.0 parts of silane coupling agent and 1.0 parts of alcohol ester dodecahydrate;

[0080] The second coating can be mixed with 25 parts of modified anionic emulsified asphalt, 55 parts of nitrile latex, 15 parts of slurry, 0.4 parts of silicone defoamer, 0.6 parts of calcium sulfate, 1.6 parts of hindered aminophenol antioxidant 1010, 2.0 parts of silane coupling agent and 1.0 parts of alcohol ester dodecahydrate;

[0081] The second coating can be mixed with 25 parts of modified anionic emulsified asphalt, 55 parts of butyl latex, 15 parts of slurry, 0.4 parts of silicone defoamer, 0.6 parts of calcium sulfate, 1.6 parts of hindered aminophenol antioxidant 1010, 2.0 parts of silane coupling agent and 1.0 parts of alcohol ester dodecahydrate;

[0082] Those skilled in the art can make settings according to requirements, and the embodiments of the present application will not be described in detail.

[0083] Based on the same inventive concept, the present invention provides a method for preparing any of the above-mentioned water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coatings. Figure 1 , Figure 1 The present invention is a flowchart of a method for preparing a water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating according to an embodiment of the present invention, comprising:

[0084] S1, preparing a first coating, comprising:

[0085] S11, heating the base asphalt to 140-160° C., stirring for 10-20 minutes, adding the filler oil and the modifier, further heating to 160-180° C., stirring for more than 4 hours, to obtain the first modified asphalt;

[0086] S12, mixing the emulsifier soap solution with the first modified asphalt, and then emulsifying the mixture by high-speed shearing in a colloid mill to obtain a modified emulsified asphalt;

[0087] S13, mixing 30-60 parts of the modified emulsified asphalt with 30-60 parts of a polymer emulsion, 3-10 parts of a tackifying resin, 5-30 parts of a filler, 0.5-2.0 parts of a defoaming agent and 0.5-3.0 parts of a thickener according to a certain proportion and stirring for 30 minutes to obtain the first coating;

[0088] According to the physical and chemical properties of each component in the first coating, it is necessary to evenly mix the components in the first coating to avoid moisture and bubbles in the system. First, it is necessary to prepare the substrate modified emulsified asphalt in the first coating, and then mix the components required for the first coating in proportion, and stir for 30 minutes to evenly mix the components in the first coating. Among them, the proportions of the components in the first coating are: 30-60 parts of polymer emulsion, 3-10 parts of tackifying resin, 5-30 parts of filler, 0.5-2.0 parts of defoamer and 0.5-3.0 parts of thickener.

[0089] Among them, the steps of preparing modified emulsified asphalt are as follows: first, 50-70 parts of base asphalt are heated to 140-160°C according to the ratio to make the base asphalt liquid, and after stirring evenly, 5-10 parts of filler oil and 1-3 parts of modifier are added, and the temperature is further raised to 160-180°C, and stirred for more than 4 hours to obtain a first modified asphalt; then, 0.5-3.0 parts of emulsifier are dissolved in an appropriate amount of water, heated to 55-70°C to obtain an emulsifier soap solution, the emulsifier soap solution is mixed with 50-70 parts of the first modified asphalt, and the mixed system of the emulsifier soap solution and the first modified asphalt is emulsified by high-speed shearing through a colloid mill to obtain a modified emulsified asphalt. Wherein, the filler oil is at least one of cycloparaffin oil and aromatic oil; the modifier is at least one of styrene-butadiene rubber and SBS rubber. In the embodiment of the present application, a polymer is preferably used as a modifier to modify the matrix asphalt to reduce its water absorption rate; since the modifier is solid, in order to completely melt the solid modifier in the matrix asphalt, the temperature needs to be further increased to 160-180°C, stirred for more than 4 hours, until the solid modifier is completely melted in the matrix asphalt, and the first modified asphalt is obtained. Then, an emulsifier soap solution is used to mix with the first modified asphalt; wherein the emulsifier is an anionic emulsifier and a nonionic emulsifier, preferably, the embodiment of the present application selects at least one of rosin and its derivatives, sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, polyoxyethylene ether, and octylphenol polyoxyethylene ether as an emulsifier, dissolves the emulsifier in an appropriate amount of water, heats to 55-70°C, forms an emulsifier soap solution, and then mixes the emulsifier soap solution with the first modified asphalt and performs high-speed shear emulsification through a colloid mill to obtain a modified emulsified asphalt.

[0090] S2, preparing a second coating, comprising:

[0091] S21, adding a dispersant, fumed silica, a filler and a defoamer into deionized water, stirring evenly, and grinding and dispersing with a grinder to obtain a slurry;

[0092] S22, 10-50 parts of the slurry, 20-70 parts of modified emulsified asphalt, 30-70 parts of latex, 0.5-2.0 parts of defoaming agent, 0.5-3.0 parts of stabilizer, 0.5-2.0 parts of UV resistant additive, 1-3 parts of coupling agent and 1-3 parts of film-forming additive are mixed and stirred in proportion for 30 minutes to obtain the second coating.

[0093] According to the physical and chemical properties of each component in the second coating, it is necessary to evenly mix the components in the second coating to avoid moisture and bubbles in the system. First, prepare the component slurry in the second coating, then mix the components required for the second coating in proportion, and stir for 30 minutes to evenly mix the components in the second coating. Among them, the proportions of the components in the second coating are: 20-70 parts of modified emulsified asphalt, 30-70 parts of latex, 10-50 parts of slurry, 0.5-2 parts of defoamer, 0.5-3.0 parts of stabilizer, 0.5-2.0 parts of UV-resistant additive, 1-3 parts of coupling agent and 1-3 parts of film-forming additive.

[0094] Among them, the steps of preparing the slurry are: first, add 3-6 parts of dispersant to 20-70 parts of deionized water, stir evenly, and obtain a dispersant system; then, add 1-3 parts of fumed silica to the dispersant system and stir evenly; then, add 20-70 parts of filler, stir at high speed, add 0.2-3.0 parts of defoamer, and grind with a grinder to obtain a slurry. In an embodiment of the present application, the dispersant is a polymer dispersant; the fumed silica is preferably hydrophilic silica. In an embodiment of the present application, the filler is preferably an inorganic hydrophobic filler, because the non-polar long chain on the surface of the inorganic hydrophobic filler blocks the contact between the second coating and water, which can significantly reduce the water absorption rate of the second coating.

[0095] The embodiment of the present application provides an application of a water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating, wherein a first coating is applied to the surface of a base material to form a first coating film, and a second coating is applied to the surface of the first coating film to form a second coating film. Preferably, the first coating is applied to the surface of the base material in a single-component application manner, and the second coating is applied to the surface of the first coating film in a two-component spraying manner; wherein the second coating and a curing agent are mixed and applied to the surface of the first coating film in a two-component spraying manner, and the curing agent can enhance the curing reaction of the second coating and enable it to form a film quickly; in the embodiment of the present application, the curing agent is preferably a metal salt solution, and specifically, it can be preferably at least one of zinc sulfate, zinc acetate, and calcium chloride. The first coating film and the second coating film form a compatible composite coating film, wherein the single-component application method allows the first coating to penetrate into the base surface more easily, so that the first coating has a higher bonding strength, and further improves the bonding force between the first coating and the second coating; since the first coating seals part of the dust in the base, the requirements for the base surface are reduced; since the first coating also contains a modified emulsified asphalt component after being applied to the base surface, the first coating has good compatibility with the second coating, so that the composite coating film has a higher bonding force.

[0096] The thickness of the first coating film is 0.1-0.4 mm, and the thickness of the second coating film is 1.5-2.5 mm.

[0097] Illustratively, the thickness of the first coating film may be 0.1 mm, 0.2 mm, 0.3 mm, 0.4 mm, etc.; the thickness of the second coating film may be 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2.0 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, etc.; those skilled in the art may set it according to needs, and the embodiments of the present application will not be elaborated in detail.

[0098] In the embodiment of the present application, the thickness of the first coating film is preferably 0.2 mm, and the thickness of the second coating film is preferably 2.0 mm.

[0099] The above preparation method is described in detail below through a number of examples.

[0100] The components in the first coating embodiment are as follows (by weight 100):

[0101] Example A1: modified emulsified asphalt, 30 parts; acrylic emulsion, 30 parts; rosin resin, 10 parts; calcium carbonate, 25 parts; BYK-018, 2.0 parts; cellulose thickener, 3.0 parts.

[0102] Example A2: modified emulsified asphalt, 35 parts, aqueous epoxy emulsion, 30 parts; terpene resin, 5 parts, calcium carbonate, 25 parts, BYK-018, 2.0 parts, cellulose thickener, 3.0 parts.

[0103] The components in the second coating embodiment are as follows (by weight 100):

[0104] Example B1: modified anionic emulsified asphalt, 30 parts; chloroprene rubber latex, 50 parts; slurry, 15 parts; BYK-018, 0.5 parts; calcium sulfate, 0.5 parts; hindered aminophenol antioxidant 1010, 1.5 parts; KH550, 1.5 parts; alcohol ester dodecahydrate, 1.5 parts.

[0105] Example B2: modified anionic emulsified asphalt, 55 parts; acrylic emulsion, 30 parts; slurry 10 parts; BYK-018, 0.3 parts; calcium sulfate, 0.7 parts; UV-resistant additive 5151, 1.7 parts; KH550, 2.0 parts; alcohol ester dodecahydrate, 1.0 parts.

[0106] Example B3: modified anionic emulsified asphalt, 25 parts; chloroprene rubber latex, 20 parts; styrene-butadiene rubber latex, 20 parts; acrylic emulsion, 20 parts; slurry, 10 parts; BYK-018, 0.4 parts; calcium sulfate, 0.6 parts; UV-resistant additive 5151, 1.6 parts; coupling agent KH550, 2.0 parts; alcohol ester dodecahydrate, 1.0 parts.

[0107] Example B4: modified anionic emulsified asphalt, 25 parts; acrylic emulsion, 45 parts; chloroprene rubber latex, 10 parts; slurry, 15 parts; BYK-018, 0.4 parts; calcium sulfate, 0.6 parts; UV-resistant additive 5151, 1.6 parts; coupling agent KH550, 2.0 parts; alcohol ester dodecahydrate, 1.0 parts.

[0108] As shown in the following Table 1, Table 1 shows the proportions of the components in Examples A1-A2 of the first coating and Examples B1-B4 of the second coating.

[0109] Table 1 Example formulation (calculated by weight 100)

[0110]

[0111] The preparation process of the first coating in Example A1-A2 in Table 1 is as follows:

[0112] First, a modified emulsified asphalt is prepared. The base asphalt is added to a reaction kettle, heated to 140-160°C, stirred for 10-20 minutes, and then the filler oil and the modifier are added. The temperature is further raised to 160-180°C, and stirred for more than 4 hours to obtain a first modified asphalt. Then, the emulsifier soap solution is mixed with the first modified asphalt, and then the emulsified product is emulsified by high-speed shearing in a colloid mill to obtain a modified emulsified asphalt.

[0113] The modified emulsified asphalt, polymer emulsion, tackifying resin, filler, defoamer and thickener were added into a stirring kettle in proportion, mixed and stirred for 30 minutes to prepare the first coating.

[0114] The preparation process of the second coating in Examples B1-B4 in Table 1 is as follows:

[0115] Firstly, a slurry is prepared, a dispersant, fumed silica, a filler, a defoamer and deionized water are added into a stirring kettle, stirred evenly, and then ground and dispersed by a grinder to obtain the slurry;

[0116] Then, the slurry, modified emulsified asphalt, latex, defoamer, stabilizer, UV-resistant additive, coupling agent and film-forming additive were added into a stirring kettle in proportion, mixed and stirred for 30 minutes to prepare a second coating.

[0117] In practical applications, after the first coating is applied to the surface of the base layer to form a first coating film, the second coating film is then applied to the first coating film to form a second coating film. Among them, the composite coating embodiment 1 in the embodiment of the present application is prepared by compounding the first coating A1 and the second coating B1; the composite coating embodiment 2 is prepared by compounding the first coating A1 and the second coating B2; the composite coating embodiment 3 is prepared by compounding the first coating A1 and the second coating B3; the composite coating embodiment 4 is prepared by compounding the first coating A1 and the second coating B4; and the composite coating embodiments 1-4 and the comparative example (the coating used in the comparative example is a common type of rubber asphalt waterproof coating) are immersed in water for 30 days and then tested, and the test results are shown in Table 2.

[0118] Table 2 Composite coating examples 1-4 and comparative examples performance test results

[0119]

[0120] Combining Table 1 and Table 2, it can be seen that the water absorption rate of the common rubber asphalt waterproof coating available on the market is as high as 4.5%, and the bonding performance with the base surface is as low as 0.54 MPa. The water absorption rate of the composite coating prepared in Examples 1-4 of the present application is the highest at 2.2%, and the bonding performance is the lowest at 0.82MPa, indicating that the water-resistant bonding spray quick-setting liquid rubber waterproof composite coating prepared in the present application can significantly reduce the water absorption rate of the composite coating and increase the bonding performance between the composite coating and the base surface. This is because the first coating and the second coating in the present application use modified emulsified asphalt with significantly reduced water absorption; further, a polymer emulsion with low water absorption is used in the first coating, and a latex with low water absorption is used in the second coating; in addition, components such as tackifying resin that can improve the bonding performance between the composite coating and the base surface are added; wherein the filler is an inorganic hydrophobic filler, which can block the contact between the composite coating and water, the addition of the defoaming agent eliminates bubbles, bubbling and other phenomena in the preparation process of the composite coating, the thickener makes the composite coating have good storage stability, the UV-resistant additive can extend the service life of the composite coating, and the coupling agent and the film-forming additive can improve the bonding strength of the composite coating and the strength and density of the composite coating.

[0121] Among them, compared with Examples 1-3, Example 4 has the lowest water absorption, which can reduce the water absorption of the composite coating to 1.5%, and Example 4 has the best bonding performance, which can improve the bonding performance of the composite coating to 1.0MPa. This is because the latex in Example 4 is selected to mix acrylic emulsion and chloroprene rubber latex, while the latex in Example 1 is only chloroprene rubber latex, the latex in Example 2 is only acrylic emulsion, and the latex in Example 3 is a mixture of chloroprene rubber latex, styrene-butadiene rubber latex and acrylic emulsion, indicating that only using a single latex with low water absorption in the composite coating cannot achieve the best effect, and only by mixing the demulsifiable acrylic emulsion with low water absorption and the chloroprene rubber latex with low water absorption in an appropriate proportion can the best effect be achieved. In addition, in the second coating, the addition ratio of modified emulsified asphalt and mixed latex should be that the weight percentage of latex is greater than the weight percentage of modified emulsified asphalt. When the amount of modified emulsified asphalt added is more than the latex, the water absorption rate of the composite coating will increase and the bonding performance will be lower (see the performance test results of Example 2 and Example 4 in Table 2). This is also the reason why although Example 2 also uses mixed latex (chloroprene rubber latex, styrene-butadiene rubber latex and acrylic emulsion), its overall performance is slightly worse than that of Example 4.

[0122] In summary, the water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating of the present invention has good comprehensive performance and can be used for the surface of the base layer in an immersion environment.

[0123] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0124] The above is a detailed introduction to a water-resistant, adhesive spray-coated quick-setting liquid rubber waterproof composite coating, a preparation method and an application thereof provided by the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for general technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating, characterized in that: The water-resistant bonding spray-coated quick-setting liquid rubber waterproof composite coating consists of a first coating and a second coating; Wherein, based on 100 parts by weight, the first coating is mixed with 30-60 parts of modified emulsified asphalt, 30-60 parts of polymer emulsion, 3-10 parts of tackifying resin, 5-30 parts of filler, 0.5-2.0 parts of defoaming agent and 0.5-3.0 parts of thickener; Based on 100 parts by weight, the second coating is mixed with 20-70 parts of modified emulsified asphalt, 30-70 parts of latex, 10-50 parts of slurry, 0.5-2.0 parts of defoamer, 0.5-3.0 parts of stabilizer, 0.5-2.0 parts of UV-resistant additive, 1-3 parts of coupling agent and 1-3 parts of film-forming additive, and the slurry is mixed with 3-6 parts of dispersant, 20-70 parts of deionized water, 1-3 parts of hydrophilic fumed silica, 20-70 parts of filler and 0.2-3.0 parts of defoamer; The filler oil is at least one of naphthenic oil and aromatic oil; the modifier is at least one of styrene-butadiene rubber and SBS rubber; the latex is at least one of chloroprene rubber latex, styrene-butadiene rubber latex, natural latex, acrylic emulsion, nitrile latex and butyl latex; the polymer emulsion is acrylic emulsion; The modified emulsified asphalt is obtained by reacting 50-70 parts of a first modified asphalt and 0.5-3.0 parts of an emulsifier, and the first modified asphalt is obtained by reacting 50-70 parts of a base asphalt, 5-10 parts of an extender oil and 1-3 parts of a modifier; the modified emulsified asphalt is prepared by the following process: heating the base asphalt to 140-160°C, stirring for 10-20 minutes, adding the extender oil and the modifier, further heating to 160-180°C, stirring for more than 4 hours, to obtain the first modified asphalt; after mixing the emulsifier soap solution with the first modified asphalt, high-speed shearing emulsification is performed by a colloid mill to obtain the modified emulsified asphalt; When the water-resistant bonding spray quick-setting liquid rubber waterproof composite coating is applied, a first coating is applied to the surface of a base layer to form a first coating film, and a second coating is applied to the surface of the first coating film to form a second coating film.

2. The composite coating according to claim 1, characterized in that: The emulsifier is an anionic emulsifier or a nonionic emulsifier.

3. The composite coating according to claim 1, characterized in that: The tackifying resin is at least one of coumarone resin, terpene resin, rosin resin and petroleum resin; The filler is at least one of calcium carbonate, barium sulfate, titanium dioxide, and silicon powder; The defoamer is a silicone defoamer; The thickener is at least one of a cellulose thickener and a water-soluble acrylic thickener.

4. The composite coating according to claim 1, characterized in that: The dispersant is a polymer dispersant; The filler is at least one of calcium bicarbonate, calcium carbonate, barium sulfate, titanium dioxide, and silicon powder; The defoaming agent is a silicone defoaming agent.

5. The composite coating according to claim 1, characterized in that: The defoamer is a silicone defoamer; The stabilizer is at least one of a vinyl silane coupling agent and calcium sulfate; The UV-resistant additive is at least one of the following: an antioxidant selected from the group consisting of aminophenols, salicylates, and benzophenones; The coupling agent is at least one of a titanate coupling agent, a silane coupling agent, and an aluminate coupling agent; The film-forming aid is at least one of alcohol ester dodecanedione, propylene glycol butyl ether, and ethylene glycol.

6. The composite coating according to claim 1, characterized in that: The first coating is prepared by mixing 30-35 parts of modified emulsified asphalt, 30 parts of polymer emulsion, 5-10 parts of tackifying resin, 25 parts of filler, 2 parts of defoamer and 3 parts of thickener; The second coating is mixed with 25-55 parts of modified emulsified asphalt, 30-60 parts of latex, 10-15 parts of slurry, 0.3-0.5 parts of defoamer, 0.5-3.0 parts of stabilizer, 1.5-1.7 parts of UV-resistant additive, 1.5-2.0 parts of coupling agent and 1.0-1.5 parts of film-forming additive.

7. The composite coating according to claim 1, characterized in that: The first coating is prepared by mixing 30 parts of modified emulsified asphalt, 30 parts of polymer emulsion, 10 parts of tackifying resin, 25 parts of filler, 2 parts of defoamer and 3 parts of thickener; The second coating is mixed with 25 parts of modified emulsified asphalt, 55 parts of latex, 15 parts of slurry, 0.4 parts of defoamer, 0.6 parts of stabilizer, 1.6 parts of UV-resistant additive, 2.0 parts of coupling agent and 1.0 parts of film-forming additive.

8. A method for preparing a water-resistant adhesive spray-coated quick-setting liquid rubber waterproof composite coating according to any one of claims 1 to 7, characterized in that: include: S1, preparing a first coating, comprising: S11, heating the base asphalt to 140-160°C, stirring for 10-20 min, adding the filler oil and the modifier, further heating to 160-180°C, stirring for more than 4 h, to obtain the first modified asphalt; S12, mixing the emulsifier soap solution with the first modified asphalt, and then emulsifying the mixture by high-speed shearing in a colloid mill to obtain a modified emulsified asphalt; S13, mixing 30-60 parts of the modified emulsified asphalt with 30-60 parts of a polymer emulsion, 3-10 parts of a tackifying resin, 5-30 parts of a filler, 0.5-2.0 parts of a defoaming agent and 0.5-3.0 parts of a thickener according to a certain proportion and stirring for 30 minutes to obtain the first coating; S2, preparing a second coating, comprising: S21, adding a dispersant, fumed silica, a filler and a defoamer into deionized water, stirring evenly, and grinding and dispersing with a grinder to obtain a slurry; S22, 10-50 parts of the slurry, 20-70 parts of the modified emulsified asphalt, 30-70 parts of the latex, 0.5-2.0 parts of the defoamer, 0.5-3.0 parts of the stabilizer, 0.5-2.0 parts of the UV-resistant additive, 1-3 parts of the coupling agent and 1-3 parts of the film-forming additive are mixed and stirred in proportion for 30 minutes to obtain the second coating.

9. An application of the water-resistant bonding spray quick-setting liquid rubber waterproof composite coating according to any one of claims 1 to 7, characterized in that: A first coating is applied to the surface of a base layer to form a first coating film, and a second coating is applied to the surface of the first coating film to form a second coating film.

10. The use according to claim 9, characterized in that The thickness of the first coating film is 0.1-0.4 mm, and the thickness of the second coating film is 1.5-2.5 mm.