A nickel paste for barium titanate-based MLCC with reduced dielectric loss and a preparation method thereof
By using additives such as triphenyl antimony diacetate and antimony pentoxide in the nickel slurry of multilayer ceramic capacitors to absorb reducing gases in the gaps, the problem of void formation during sintering of the nickel slurry and the barium titanate dielectric layer is solved. , reducing dielectric loss and improving capacitance and reliability.
Patent Information
- Application Number
- CN202310642069.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-01
AI Technical Summary
In the manufacturing process of multilayer ceramic capacitors, gaps are formed due to different thermal expansion coefficients during the sintering of the nickel slurry and the barium titanate dielectric layer. The reducing gas in the gaps is difficult to discharge, resulting in increased dielectric loss, decreased resistivity, and leakage current. problems such as increase in capacitance and reduced reliability.
The formula using nickel slurry includes nickel powder, inorganic binder, organic binder, organic additives and inorganic additives. Through the synergistic effect of antimony triphenyl diacetate and antimony pentoxide, the reducing gas in the voids is absorbed. , prevent barium titanate from being reduced or semiconducted, thereby densifying the nickel slurry and dielectric layer, reducing dielectric loss and improving capacitance and reliability.
It effectively reduces dielectric loss, improves capacitance and reliability, prevents the reduction or semiconductorization of barium titanate, promotes the densification of nickel slurry and dielectric layers, and improves the electrical performance and reliability of MLCC.
Smart Images

Figure BDA0004261830480000121 
Figure BDA0004261830480000131
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nickel paste for multilayer ceramic capacitors, and in particular relates to a nickel paste for barium titanate-based MLCC with reduced dielectric loss and a preparation method thereof. Background Art
[0002] Multi-layer ceramic capacitors (MLCC) are mainly composed of ceramic dielectric films, metal inner electrodes, and metal outer electrodes. MLCC is made by alternately stacking ceramic dielectric films printed with metal inner electrodes and sintering them at high temperatures to form a ceramic chip, and then encapsulating metal outer electrodes at both ends of the chip. The production process mainly includes batching, casting, printing, stacking, lamination, cutting, debinding, sintering, chamfering, capping, burning, electroplating, testing, etc. MLCC has the characteristics of small size, high integration, and high reliability, and is widely used in the electronic and electrical industry.
[0003] In the process of making chip-type multilayer ceramic capacitors, nickel paste is usually printed as an internal electrode on the barium titanate ceramic dielectric film. The nickel paste and the ceramic dielectric film need to be co-fired to make the structure dense and form good contact. In order to prevent the nickel paste from being oxidized during the co-firing process and losing its function as an internal electrode, the nickel paste needs to be sintered in a reducing atmosphere such as hydrogen. However, barium titanate is prone to produce oxygen ion vacancies and semiconductorization when sintered in a reducing atmosphere, resulting in a significant decrease in resistivity. Traditional MLCC improves the reduction resistance of barium titanate dielectrics by doping anti-reduction materials in the dielectric film, such as amphoteric rare earth ion materials, transition metal ion materials, etc. However, during the process of gradual densification of the nickel paste layer and the barium titanate dielectric layer during co-firing, due to the different thermal expansion coefficients of the two, some gaps are easily generated between the nickel paste layer and the dielectric layer, and more reducing gases will be filled in the gaps. These reducing gases will cause the barium titanate component on the surface of the dielectric layer doped with anti-reduction materials to be reduced and semiconductorized during co-firing, resulting in problems such as increased leakage current, decreased resistivity, increased dielectric loss, and decreased capacitance in the MLCC. At the same time, as the nickel paste layer and the dielectric layer gradually become denser during the sintering process, the gas in the gap is difficult to discharge, and the defects caused will also reduce the reliability of the MLCC.
[0004] Invention patent CN113948235B discloses a nickel inner electrode slurry with high dispersibility and low shrinkage and its preparation method, using TiO 2 / BaCO 3 / MgO coated nickel powder, when applied to nickel internal electrode slurry, can overcome the problem of uneven dispersion of nano-BaTiO3 in the traditional nickel internal electrode production process, thereby reducing the shrinkage rate of the nickel internal electrode slurry during sintering, improving the matching of the shrinkage rate of the nickel internal electrode slurry and the MLCC cast film tape, and reducing the holes and discontinuities in the MLCC internal electrodes.
[0005] The literature [“Study on the Matching of Firing Shrinkage between Electrode Paste and Dielectric Material in Nickel Electrode MLCC”, Zhang Shaoge, Electronic Quality. 2010(04)] studied the effect of inorganic additives (such as ceramic powder) on the slurry sintering shrinkage rate. The results showed that the addition of inorganic additives to nickel internal electrode slurry can improve the shrinkage problem of the slurry before the dielectric material during the sintering process.
[0006] However, the above patents and documents only improve the shrinkage matching problem between the nickel inner electrode slurry and the dielectric material when it is fired, and do not solve the problem of reducing gas filling in the gaps formed between the nickel inner electrode slurry and the dielectric material when it is fired. That is, the above patents and documents cannot completely solve the shrinkage matching problem. The gaps in the MLCC inner electrode will still exist, but the size of the gaps is a problem. The reducing gas in the gaps will still reduce the surface of the dielectric layer, causing the MLCC to have problems such as increased leakage current, decreased resistivity, increased dielectric loss, and reduced capacitance. At the same time, the reliability of the MLCC has been reduced, and these problems have not been effectively solved. Summary of the invention
[0007] In view of the deficiencies in the prior art, the present invention provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss and a preparation method thereof, aiming to reduce dielectric loss and improve capacitance and reliability.
[0008] The specific technical solutions of the present invention are as follows:
[0009] A nickel paste for barium titanate-based MLCC with reduced dielectric loss, the nickel paste comprising the following components in parts by mass: 55-70 parts of nickel powder, 1-3 parts of inorganic binder, 25-45 parts of organic binder, 0.5-2 parts of organic additive and 0.1-1 parts of inorganic additive.
[0010] Preferably, the nickel powder is spherical, with an average particle size of 0.3-0.6 μm and a tap density of 2.2-3.4 g / cm 3 , with a specific surface area of 1-3.6m 2 / g.
[0011] Preferably, the inorganic additive is antimony pentoxide, with an average particle size of 0.05-0.2 μm and a tap density of 1.22-2.5 g / cm 3 , with a specific surface area of 3.8-6m 2 / g, melting point is 380-460℃.
[0012] Preferably, the organic auxiliary agent is triphenyl antimony diacetate, which has a melting point of 200-240°C.
[0013] Preferably, the organic binder is prepared from 35-45 parts by mass of butyl carbitol acetate, 15-25 parts by mass of acetyl tributyl citrate, 10-20 parts by mass of castor oil, 10-15 parts by mass of diffusion pump oil, 8-18 parts by mass of ethyl cellulose, 1-2 parts by mass of sorbitan trioleate and 1-2 parts by mass of polyamide wax.
[0014] Preferably, the inorganic binder is composed of 10-20 parts by mass of SiO 2 10-20 portions B 2 O 3 , 25-50 copies of Bi 2 O 3 , 8-15 parts BaCO 3 , 8-15 parts Sb2O5, 5-10 parts ZnO, 2-8 parts Mn 3 O 4 , 2-6 parts CuO and 1-4 parts TiO 2 Prepared.
[0015] The present invention also provides a method for preparing the nickel paste for barium titanate-based MLCC with reduced dielectric loss, comprising the following preparation steps:
[0016] (1) Preparation of organic binder: All raw materials for preparing the organic binder are placed in a glass reactor according to the mass ratio, stirred, and then mixed for 10-12 hours, and filtered to obtain the organic binder;
[0017] (2) Preparation of an inorganic binder: All raw materials for preparing the inorganic binder are placed in a bag and mixed evenly according to a mass ratio, and then added to a corundum crucible. The corundum crucible containing the materials is placed in a muffle furnace for smelting for 0.2-1.5 hours, and glass material is obtained after water quenching. The glass material is ball-milled for 25-40 hours, dried, and filtered to obtain an inorganic binder;
[0018] (3) Preparation of nickel slurry: Inorganic additives, organic additives and the organic binder prepared in step (1) are mixed according to the mass ratio and stirred for 0.2-1 hour, and then the inorganic binder prepared in step (2) is added and stirred for 0.2-1 hour, and then nickel powder is added and stirred for 2-6 hours. The nickel slurry is obtained after slurrying on a three-roll mill for 12-15 times.
[0019] Preferably, the organic and inorganic additives are treated by the following method before being added:
[0020] The antimony pentoxide and the molten triphenyl antimony diacetate are mixed and dispersed uniformly, and the mixture is obtained by spray drying; the two molten materials, citrus stearic acid and lithium stearate, are mixed uniformly, sprayed onto the surface of the mixture, and cooled and dried;
[0021] The added amounts of citric acid and lithium stearate are 2-5% and 4-8% of the mass of the mixture respectively.
[0022] Preferably, the stirring temperature in the glass reactor in step (1) is 80-90°C, and the smelting temperature in the muffle furnace in step (2) is 1050-1300°C.
[0023] The beneficial effects of the present invention are:
[0024] 1. The nickel paste for barium titanate-based MLCC of the present invention can effectively reduce dielectric loss, improve capacitance and reliability by controlling the formula components and preparation process of the paste.
[0025] 2. The present invention adopts triphenyl antimony diacetate as an organic auxiliary agent with a melting point of 200-240°C, which mainly acts in the early stage of co-firing. Triphenyl antimony diacetate can be dissolved in an organic binder system and evenly distributed in the nickel paste by a dispersion process. When the nickel paste is printed on the surface of the dielectric layer, the triphenyl antimony diacetate is evenly distributed on the surface of the dielectric layer and in the micropores before co-firing, so that in the early stage of co-firing, the triphenyl antimony diacetate can absorb the reducing gas in the gap between the nickel paste layer and the dielectric layer and become trivalent antimony, which plays a role in preventing the barium titanate on the surface of the dielectric layer from being reduced or semiconductorized. At the same time, the reduction of gas in the gap is conducive to shrinking the gap, and reduces the exhaust volume of the dielectric layer and the nickel paste layer, which is conducive to the densification of the dielectric layer and the nickel paste layer, and improves the reliability of MLCC.
[0026] 3. The present invention uses antimony pentoxide powder as an inorganic additive for nickel paste, with a melting point of 380-460°C, which mainly acts in the middle and late stages of co-firing. In the middle and late stages of co-firing, antimony pentoxide can melt and flow and cover and fill the surface of the dielectric layer and the micropores. It can not only absorb more reducing gases in the gaps during co-firing to form trivalent antimony, but also further prevent or reduce the reduction or semiconductorization of barium titanate on the surface of the dielectric layer, and further shrink the gaps and densify the nickel paste layer and the dielectric layer, thereby improving the electrical performance and reliability of MLCC.
[0027] 4. Under the synergistic effect of the above-mentioned organic additives and inorganic additives, the nickel paste for barium titanate-based MLCC with reduced dielectric loss prepared by the present invention can prevent or reduce the reduction or semiconductorization of barium titanate, and at the same time play a role in shrinking gaps and densifying the nickel paste layer and the dielectric layer, thereby achieving the purpose of reducing dielectric loss, improving capacitance and reliability of MLCC.
[0028] 5. Since the inorganic and organic additives in the nickel slurry are easily reduced in advance under the reducing gas sintering conditions and lose the function of absorbing the reducing gas in the pores, the present invention also treats the inorganic and organic additives before use. Specifically, the organic additive triphenyl antimony diacetate is coated on the surface of antimony pentoxide, and then citric acid (melting point 240°C) and lithium stearate (melting point 220°C) are sprayed on the surface. The treated inorganic and organic additives are prevented from being reduced in advance during the sintering process.
[0029] 6. When treating inorganic and organic additives, the combination of citric acid and lithium stearate can improve the fluidity of inorganic and organic additives in nickel slurry and promote the melting fluidity of organic additives in the early stage of sintering.
[0030] 7. When treating inorganic and organic additives, citrus fatty acid can also react with hydrogen to offset the effect of reducing hydrogen on inorganic and organic additives. Implementation
[0031] The present invention is further described below in conjunction with the embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] The present embodiment provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss, the nickel paste being made of the following components in parts by mass: 58 parts of nickel powder, 2 parts of inorganic binder, 38 parts of organic binder, 1.5 parts of organic additive triphenyl antimony diacetate, and 0.5 parts of inorganic additive antimony pentoxide.
[0034] The specifications of nickel powder are: spherical, average particle size 0.6μm, tap density 3.4g / cm 3 , specific surface area 1m 2 / g.
[0035] The specifications of antimony pentoxide are: average particle size 0.14μm, tap density 2.3g / cm 3 , specific surface area 4.5m 2 / g, melting point is 412℃.
[0036] The melting point of triphenyl antimony diacetate is 228°C.
[0037] The organic binder is prepared from 45 parts by weight of butyl carbitol acetate, 21 parts by weight of acetyl tributyl citrate, 12 parts by weight of castor oil, 10 parts by weight of diffusion pump oil, 10 parts by weight of ethyl cellulose, 1 part by weight of sorbitan trioleate and 1 part by weight of polyamide wax.
[0038] The inorganic binder is composed of 14 parts by mass of SiO 2 10 copies of B 2 O 3 , 50 copies of Bi 2 O 3 , 8 parts BaCO 3 , 8 parts ZnO, 6 parts Mn 3 O 4 , 2 parts CuO and 2 parts TiO 2 Prepared.
[0039] The preparation steps of the above nickel slurry are as follows:
[0040] (1) Preparation of organic binder: First, butyl carbitol acetate, acetyl tributyl citrate, castor oil, diffusion pump oil, ethyl cellulose, sorbitan trioleate and polyamide wax were placed in a glass reactor according to the mass ratio and stirred, then mixed at a stirring temperature of 80° C. for 10 hours, and finally filtered to obtain a transparent organic binder.
[0041] (2) Preparation of inorganic binder: SiO 2 , B 2 O 3 、Bi 2 O 3 、BaCO 3 , ZnO, Mn 3 O 4 , CuO and TiO 2 Put them in a bag, mix them evenly and add them to a corundum crucible. Put the corundum crucible with the materials in a muffle furnace and smelt them at 1200°C for 1 hour. After water quenching, obtain glass material. Ball mill the glass material for 30 hours, dry and filter it to obtain an inorganic binder with an average particle size of 0.64 μm.
[0042] (3) Preparation of nickel slurry: Inorganic additives, organic additives and the organic binder prepared in step (1) were mixed according to the mass ratio and stirred for 0.2 hours. The inorganic binder prepared in step (2) was then added and stirred for 0.5 hours. Then nickel powder was added and stirred for 2 hours. After 12 times of slurry rolling on a three-roll mill, a nickel slurry with a viscosity of 32 kcps and a fineness of 3 μm was obtained.
[0043] Example 2
[0044] The present embodiment provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss. The nickel paste is made of the following components in parts by mass: 63 parts of nickel powder, 2 parts of inorganic binder, 33 parts of organic binder, 2 parts of organic additive triphenyl antimony diacetate, and 1 part of inorganic additive antimony pentoxide.
[0045] The specifications of nickel powder are: spherical, average particle size 0.3μm, tap density 2.5g / cm 3 , specific surface area 3.6m 2 / g.
[0046] The specifications of antimony pentoxide are: powder, average particle size 0.2μm, tap density 2.5g / cm 3 , specific surface area 3.8m 2 / g, melting point is 430℃.
[0047] The melting point of triphenyl antimony diacetate is 233°C.
[0048] The organic binder is prepared from 40 parts by weight of butyl carbitol acetate, 15 parts by weight of acetyl tributyl citrate, 10 parts by weight of castor oil, 10 parts by weight of diffusion pump oil, 18 parts by weight of ethyl cellulose, 2 parts by weight of sorbitan trioleate and 1 part by weight of polyamide wax.
[0049] The inorganic binder is composed of 20 parts by mass of SiO 2 10 copies of B 2 O 3 , 38 Bi 2 O 3 , 8 parts BaCO 3 ,, 5 parts ZnO, 5 parts Mn 3 O 4 , 3 parts CuO and 4 parts TiO 2 Prepared.
[0050] The preparation steps of the above nickel slurry are as follows:
[0051] (1) Preparation of organic binder: First, butyl carbitol acetate, acetyl tributyl citrate, castor oil, diffusion pump oil, ethyl cellulose, sorbitan trioleate and polyamide wax were placed in a glass reactor according to the mass ratio and stirred, then mixed at a stirring temperature of 80° C. for 12 hours, and finally filtered to obtain a transparent organic binder.
[0052] (2) Preparation of inorganic binder: SiO 2 , B 2 O 3 、Bi 2 O 3 、BaCO 3 , ZnO, Mn 3 O 4 , CuO and TiO 2Put them in a bag, mix them evenly and add them to a corundum crucible. Put the corundum crucible with the materials in a muffle furnace and smelt them at 1050°C for 1.5 hours. After water quenching, obtain glass material. Ball mill the glass material for 35 hours, dry and filter it to obtain an inorganic binder with an average particle size of 0.8 μm.
[0053] (3) Preparation of nickel slurry: Inorganic additives, organic additives and the organic binder prepared in step (1) were mixed according to the mass ratio and stirred for 0.5 hour, and then the inorganic binder prepared in step (2) was added and stirred for 0.5 hour, and then nickel powder was added and stirred for 2 hours. After 15 times of slurry rolling on a three-roll mill, a nickel slurry with a viscosity of 38 kcps and a fineness of 3 μm was obtained.
[0054] Example 3
[0055] The present embodiment provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss, the nickel paste being made of the following components in parts by mass: 70 parts of nickel powder, 3 parts of inorganic binder, 25 parts of organic binder, 1.8 parts of organic additive triphenyl antimony diacetate, and 0.6 parts of inorganic additive antimony pentoxide.
[0056] The specifications of nickel powder are: spherical, average particle size 0.5μm, tap density 3.0g / cm 3 , specific surface area 1.96m 2 / g.
[0057] The specifications of antimony pentoxide are: powder, average particle size 0.08μm, tap density 1.58g / cm 3 , specific surface area 5.5m 2 / g, melting point is 382℃.
[0058] The melting point of triphenyl antimony diacetate is 208°C.
[0059] The organic binder is prepared from 42 parts by weight of butyl carbitol acetate, 22 parts by weight of acetyl tributyl citrate, 13 parts by weight of castor oil, 12 parts by weight of diffusion pump oil, 8 parts by weight of ethyl cellulose, 2 parts by weight of sorbitan trioleate and 1 part by weight of polyamide wax.
[0060] The inorganic binder is composed of 10 parts by mass of SiO 2 , 20 copies B 2 O 3 , 30 copies of Bi 2 O 3 , 12 parts BaCO 3 , 6 parts ZnO, 4 parts Mn 3 O 4 , 6 parts CuO and 1 part TiO 2 Prepared.
[0061] The preparation steps of the above nickel slurry are as follows:
[0062] (1) Preparation of organic binder: First, butyl carbitol acetate, acetyl tributyl citrate, castor oil, diffusion pump oil, ethyl cellulose, sorbitan trioleate, and polyamide wax were placed in a glass reactor according to the mass ratio and stirred. Then, the mixture was mixed at a stirring temperature of 90° C. for 11 hours, and finally, the transparent organic binder was obtained by filtering.
[0063] (2) Preparation of inorganic binder: SiO 2 , B 2 O 3 、Bi 2 O 3 、BaCO 3 , ZnO, Mn 3 O 4 , CuO and TiO 2 Put them in a bag and mix them evenly, then add them into a corundum crucible. Put the corundum crucible with the materials in a muffle furnace and melt them at 1100°C for 0.6 hours. After quenching with water, glass material is obtained. The glass material is ball-milled for 28 hours, dried and filtered to obtain an inorganic binder with an average particle size of 0.56 μm.
[0064] (3) Preparation of nickel slurry: Inorganic additives, organic additives and the organic binder prepared in step (1) were mixed according to the mass ratio and stirred for 1 hour, and then the inorganic binder prepared in step (2) was added and stirred for 1 hour, and then nickel powder was added and stirred for 6 hours. After 14 times of slurry rolling on a three-roll mill, a nickel slurry with a viscosity of 47 kcps and a fineness of less than 2 μm was obtained.
[0065] Example 4
[0066] The present embodiment provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss, the nickel paste being made of the following components in parts by mass: 55 parts of nickel powder, 1 part of inorganic binder, 45 parts of organic binder, 1.5 parts of organic additive triphenyl antimony diacetate, and 0.1 parts of inorganic additive antimony pentoxide.
[0067] The specifications of nickel powder are: spherical, average particle size 0.4μm, tap density 2.7g / cm 3 , specific surface area 2.8m 2 / g.
[0068] The specifications of antimony pentoxide are: powder, average particle size 0.1μm, tap density 1.93g / cm 3 , with a specific surface area of 4.8m 2 / g, melting point is 397℃.
[0069] The melting point of triphenyl antimony diacetate is 226°C.
[0070] The organic binder is prepared from 35 parts by weight of butyl carbitol acetate, 25 parts by weight of acetyl tributyl citrate, 13 parts by weight of castor oil, 15 parts by weight of diffusion pump oil, 11 parts by weight of ethyl cellulose, 1.5 parts by weight of sorbitan trioleate and 1.5 parts by weight of polyamide wax.
[0071] The inorganic binder is composed of 18 parts by mass of SiO 2 、11 copies B 2 O 3 , 25 Bi 2 O 3 、15 parts BaCO 3 , 10 parts ZnO, 8 parts Mn 3 O 4 , 2 parts CuO and 2 parts TiO 2 Prepared.
[0072] The preparation steps of the above nickel slurry are as follows:
[0073] (1) Preparation of organic binder: First, butyl carbitol acetate, acetyl tributyl citrate, castor oil, diffusion pump oil, ethyl cellulose, sorbitan trioleate and polyamide wax were placed in a glass reactor according to the mass ratio and stirred, then mixed at a stirring temperature of 85° C. for 11 hours, and finally filtered to obtain a transparent organic binder.
[0074] (2) Preparation of inorganic binder: SiO 2 , B 2 O 3 、Bi 2 O 3 、BaCO 3 , ZnO, Mn 3 O 4 , CuO and TiO 2 Put them in a bag, mix them evenly and add them to a corundum crucible. Put the corundum crucible with the materials in a muffle furnace and smelt them at 1250°C for 0.8 hours. After water quenching, obtain glass material. Ball mill the glass material for 32 hours, dry and filter it to obtain an inorganic binder with an average particle size of 0.72 μm.
[0075] (3) Preparation of nickel slurry: Inorganic additives, organic additives and the organic binder prepared in step (1) were mixed according to the mass ratio and stirred for 0.4 hours, and then the inorganic binder prepared in step (2) was added and stirred for 0.8 hours. Then nickel powder was added and stirred for 4 hours. After 13 times of slurry rolling on a three-roll mill, a nickel slurry with a viscosity of 31 kcps and a fineness of 3 μm was obtained.
[0076] Example 5
[0077] The present embodiment provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss, the nickel paste being made of the following components in parts by mass: 60 parts of nickel powder, 2.2 parts of inorganic binder, 36 parts of organic binder, 0.5 parts of organic additive triphenyl antimony diacetate, and 0.7 parts of inorganic additive antimony pentoxide.
[0078] The specifications of nickel powder are: spherical, average particle size 0.3μm, tap density 2.6g / cm 3 , specific surface area 3.5m 2 / g.
[0079] The specifications of antimony pentoxide are: powder, average particle size 0.05μm, tap density 1.22g / cm 3 , with a specific surface area of 6m 2 / g, melting point is 380℃.
[0080] The melting point of triphenyl antimony diacetate is 205°C.
[0081] The organic binder is prepared from 39 parts by weight of butyl carbitol acetate, 23 parts by weight of acetyl tributyl citrate, 20 parts by weight of castor oil, 12 parts by weight of diffusion pump oil, 9 parts by weight of ethyl cellulose, 2 parts by weight of sorbitan trioleate and 1 part by weight of polyamide wax.
[0082] The inorganic binder is composed of 13 parts by weight of SiO 2 16 copies of B 2 O 3 , 40 copies of Bi 2 O 3 , 8 parts BaCO 3 , 8 parts ZnO, 2 parts Mn 3 O 4 , 2 parts CuO and 1 part TiO 2 Prepared.
[0083] The preparation steps of the above nickel slurry are as follows:
[0084] (1) Preparation of organic binder: First, butyl carbitol acetate, acetyl tributyl citrate, castor oil, diffusion pump oil, ethyl cellulose, sorbitan trioleate, and polyamide wax were placed in a glass reactor according to the mass ratio and stirred, then mixed at a stirring temperature of 86° C. for 10 hours, and finally filtered to obtain a transparent organic binder.
[0085] (2) Preparation of inorganic binder: SiO 2 , B 2 O 3 、Bi 2 O 3 、BaCO 3 , ZnO, Mn3 O 4 , CuO and TiO 2 Put them in a bag, mix them evenly and add them to a corundum crucible. Put the corundum crucible with the materials in a muffle furnace and smelt them at 1300°C for 0.2 hours. After water quenching, obtain glass material. Ball mill the glass material for 28 hours, dry and filter it to obtain an inorganic binder with an average particle size of 0.52 μm.
[0086] (3) Preparation of nickel slurry: Inorganic additives, organic additives and the organic binder prepared in step (1) were mixed according to the mass ratio and stirred for 0.4 hours, and then the inorganic binder prepared in step (2) was added and stirred for 1 hour, and then nickel powder was added and stirred for 5 hours. After 15 times of slurry rolling on a three-roll mill, a nickel slurry with a viscosity of 42 kcps and a fineness of less than 2 μm was obtained.
[0087] Example 6
[0088] On the basis of Example 1, this embodiment further provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss, wherein the organic additives and inorganic additives used are treated by the following method and then added:
[0089] Antimony pentoxide and molten triphenyl antimony diacetate are mixed and dispersed uniformly, and then spray-dried to obtain a mixture one; two molten materials, citrus fatty acid and lithium stearate, are mixed uniformly, sprayed onto the surface of the mixture one, and cooled and dried; the amounts of citrus fatty acid and lithium stearate added are 2% and 8% of the mass of the mixture one (i.e., the total mass of antimony pentoxide and triphenyl antimony diacetate), respectively.
[0090] The rest is the same as Example 1.
[0091] Example 7
[0092] On the basis of Example 2, this embodiment also provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss. The organic and inorganic additives used are treated before being added. The treatment steps are the same as those in Example 1. The amounts of citric acid and lithium stearate added are 3% and 6% of the mass of the mixture, respectively.
[0093] Example 8
[0094] On the basis of Example 2, this embodiment also provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss. The organic and inorganic additives used are treated before being added. The treatment steps are the same as those in Example 1. The amounts of citric acid and lithium stearate added are 5% and 4% of the mass of the mixture, respectively.
[0095] Example 9
[0096] On the basis of Example 2, this embodiment also provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss. The organic and inorganic additives used are treated before being added. The treatment steps are the same as those in Example 1. The amounts of citric acid and lithium stearate added are 2% and 7% of the mass of the mixture, respectively.
[0097] Example 10
[0098] On the basis of Example 2, this embodiment also provides a nickel paste for barium titanate-based MLCC with reduced dielectric loss. The organic and inorganic additives used are treated before being added. The treatment steps are the same as those in Example 1. The amounts of citric acid and lithium stearate added are 4% and 6% of the mass of the mixture, respectively.
[0099] Comparative Example 1
[0100] The difference between this comparative example and Example 1 is that the components of the nickel slurry do not contain the organic auxiliary agent triphenyl antimony diacetate and the inorganic auxiliary agent antimony pentoxide.
[0101] Comparative Example 2
[0102] The difference between this comparative example and Example 1 is that the nickel slurry does not contain the inorganic auxiliary agent antimony pentoxide.
[0103] Comparative Example 3
[0104] The difference between this comparative example and Example 1 is that the components of the nickel slurry do not contain the organic auxiliary agent triphenyl antimony diacetate.
[0105] Comparative Example 4
[0106] The difference between this comparative example and Example 1 is that the organic auxiliary agent triphenyl antimony diacetate in the nickel slurry component is replaced by the dispersant Hypermer KD-9.
[0107] Comparative Example 5
[0108] The difference between this comparative example and Example 1 is that the organic auxiliary agent triphenyl antimony diacetate in the nickel paste component is replaced by antimony acetate.
[0109] Comparative Example 6
[0110] The difference between this comparative example and Example 1 is that the inorganic auxiliary agent antimony pentoxide in the nickel paste component is replaced by ceramic powder.
[0111] Comparative Example 7
[0112] The difference between this comparative example and Example 1 is that the inorganic auxiliary agent antimony pentoxide in the nickel slurry component is replaced by antimony trioxide.
[0113] Comparative Example 8
[0114] The difference between this comparative example and Example 1 is that the mass fraction of the organic auxiliary agent triphenyl antimony diacetate in the nickel paste component is 0.3 parts.
[0115] Comparative Example 9
[0116] The difference between this comparative example and Example 1 is that the mass fraction of the organic auxiliary agent triphenyl antimony diacetate in the nickel slurry component is 2.2 parts.
[0117] Comparative Example 10
[0118] The difference between this comparative example and Example 1 is that the mass fraction of the inorganic auxiliary agent antimony pentoxide in the nickel paste component is 0.05 parts.
[0119] Comparative Example 11
[0120] The difference between this comparative example and Example 1 is that the mass fraction of the inorganic auxiliary agent antimony pentoxide in the nickel paste component is 1.1 parts.
[0121] Comparative Example 12
[0122] The difference between this comparative example and Example 6 is that in the preparation step of the nickel slurry, the inorganic additive is not treated, and only the organic additive triphenyl antimony diacetate is treated by the following method before being added: the two molten materials, citrus stearic acid and lithium stearate, are mixed evenly, sprayed onto the surface of triphenyl antimony diacetate, and cooled and dried.
[0123] Comparative Example 13
[0124] The difference between this comparative example and Example 6 is that in the preparation step of the nickel slurry, the organic additive is not treated, and only the inorganic additive antimony pentoxide is treated by the following method before being added: the two molten materials, citrus stearic acid and lithium stearate, are mixed evenly, sprayed onto the surface of the antimony pentoxide, and cooled and dried.
[0125] Comparative Example 14
[0126] The difference between this comparative example and Example 6 is that in the preparation step of the nickel slurry, the organic additive and the inorganic additive are treated by the following method before being added: antimony pentoxide and triphenyl antimony diacetate are mixed and dispersed uniformly to obtain a mixture 1; the two molten materials, citrus stearic acid and lithium stearate, are mixed uniformly, sprayed onto the surface of the mixture 1, and cooled and dried.
[0127] Comparative Example 15
[0128] The difference between this comparative example and Example 6 is that in the preparation step of the nickel slurry, the organic additive and the inorganic additive are treated by the following method before being added: molten antimony pentoxide is sprayed onto the surface of triphenyl antimony diacetate, and a mixture is obtained by cooling and drying; the two molten materials, citrus stearic acid and lithium stearate, are mixed evenly, and then sprayed onto the surface of the mixture, and then cooled and dried.
[0129] Comparative Example 16
[0130] The difference between this comparative example and Example 6 is that in the step of preparing the nickel slurry, the organic additive and the inorganic additive are treated by the following method before being added: antimony pentoxide and molten triphenyl antimony diacetate are mixed and dispersed uniformly, and a mixture is obtained by spray drying.
[0131] Comparative Example 17
[0132] The difference between this comparative example and Example 6 is that in the step of preparing the nickel slurry, the organic additive and the inorganic additive are treated by the following method before being added: antimony pentoxide and molten triphenyl antimony diacetate are mixed and dispersed uniformly, and a mixture is obtained by spray drying; and molten citrus fatty acid is sprayed onto the surface of the mixture, and the mixture is cooled and dried.
[0133] Comparative Example 18
[0134] The difference between this comparative example and Example 6 is that in the preparation step of the nickel slurry, the organic additive and the inorganic additive are treated by the following method before being added: antimony pentoxide and molten triphenyl antimony diacetate are mixed and dispersed uniformly, and a mixture is obtained by spray drying; and molten lithium stearate is sprayed onto the surface of the mixture, and the mixture is cooled and dried.
[0135] Comparative Example 19
[0136] The difference between this comparative example and Example 6 is that the amount of citric acid added is 1% by mass of the mixture.
[0137] Comparative Example 20
[0138] The difference between this comparative example and Example 6 is that the amount of citric acid added is 6% by mass of the mixture.
[0139] Comparative Example 21
[0140] The difference between this comparative example and Example 6 is that the amount of lithium stearate added is 3% by mass of the mixture.
[0141] Comparative Example 22
[0142] The difference between this comparative example and Example 6 is that the amount of lithium stearate added is 9% of the mass of the mixture. 1. Electrical performance and reliability test of MLCC products
[0143] The nickel pastes prepared in Examples 1-10 and Comparative Examples 1-22 of the present invention were applied to barium titanate-based MLCC products. The electrical properties and reliability of the products were tested in accordance with GB / T21042-2007 and highly accelerated life test standards. The results are shown in Table 1 below.
[0144] Table 1 Electrical performance and reliability test results of MLCC products
[0145]
[0146]
[0147] From the results in Table 1, it can be seen that the electrical properties and reliability of the MLCC products made of nickel paste in Examples 1-5 of the present invention are significantly better than those in Comparative Examples 1-11, indicating that the use of antimony pentoxide and triphenyl antimony diacetate as inorganic and organic additives of nickel paste in the present invention is beneficial to reducing the dielectric loss of barium titanate-based MLCC products, and at the same time plays a role in improving capacitance and reliability, and the addition amount of antimony pentoxide and triphenyl antimony diacetate needs to be controlled within a reasonable range.
[0148] On the basis of Examples 1-5, in Examples 6-10, antimony pentoxide and triphenyl antimony diacetate were treated and then added to the nickel paste. As a result, the capacitance value was significantly improved, the dielectric loss was reduced, and the electrical performance of the MLCC product was further improved.
[0149] Compared with Example 6, Comparative Examples 12-22 respectively changed the treatment methods of antimony pentoxide and triphenyl antimony diacetate, and as a result, the electrical properties decreased to varying degrees, and the reliability of some comparative examples also decreased, indicating that antimony pentoxide and triphenyl antimony diacetate need to be treated according to the method of the present invention in order to more effectively improve the electrical properties and reliability.
[0150] It is worth noting that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection of the present invention.
Claims
1. A nickel paste for barium titanate-based MLCC with reduced dielectric loss, Features: The nickel paste comprises the following components in parts by weight: 55-70 parts of nickel powder, 1-3 parts of inorganic binder, 25-45 parts of organic binder, 0.5-2 parts of organic additive and 0.1-1 parts of inorganic additive; The inorganic auxiliary agent is antimony pentoxide; The organic auxiliary agent is triphenyl antimony diacetate.
2. The nickel paste for barium titanate-based MLCC with reduced dielectric loss according to claim 1, Features: The nickel powder is spherical, with an average particle size of 0.3-0.6 μm and a tap density of 2.2-3.4 g / cm 3 , with a specific surface area of 1-3.6m 2 / g.
3. The nickel paste for barium titanate-based MLCC with reduced dielectric loss according to claim 1, Features: The organic binder is prepared from 35-45 parts by weight of butyl carbitol acetate, 15-25 parts by weight of acetyl tributyl citrate, 10-20 parts by weight of castor oil, 10-15 parts by weight of diffusion pump oil, 8-18 parts by weight of ethyl cellulose, 1-2 parts by weight of sorbitan trioleate and 1-2 parts by weight of polyamide wax.
4. The nickel paste for barium titanate-based MLCC with reduced dielectric loss according to claim 1, Features: The inorganic binder is composed of 10-20 parts by mass of SiO 2 10-20 portions B 2 O 3 , 25-50 copies of Bi 2 O 3 , 8-15 parts BaCO 3 , 5-10 parts ZnO, 2-8 parts Mn 3 O 4 , 2-6 parts CuO and 1-4 parts TiO 2 Prepared.
5. The nickel paste for barium titanate-based MLCC with reduced dielectric loss according to claim 1, Features: The average particle size of the antimony pentoxide is 0.05-0.2 μm, and the tap density is 1.22-2.5 g / cm 3 , with a specific surface area of 3.8-6m 2 / g.
6. A method for preparing nickel paste for barium titanate-based MLCC with reduced dielectric loss according to claim 1, Features: The method comprises the following preparation steps: (1) Preparation of organic binder: Place all the raw materials for preparing the organic binder in a glass reactor according to the mass ratio, stir, mix for 10-12 hours, and filter to obtain the organic binder; (2) Preparation of inorganic binder: All raw materials for preparing the inorganic binder are mixed uniformly according to the mass ratio and placed in a muffle furnace for smelting for 0.2-1.5 hours. After water quenching, glass material is obtained. The glass material is ball-milled for 25-40 hours, dried and filtered to obtain the inorganic binder; (3) Preparation of nickel slurry: Inorganic additives, organic additives and the organic binder prepared in step (1) are mixed according to the mass ratio and stirred for 0.2-1 hour, and then the inorganic binder prepared in step (2) is added and stirred for 0.2-1 hour, and then nickel powder is added and stirred for 2-6 hours. The nickel slurry is obtained after slurrying on a three-roll mill for 12-15 times.
7. The method for preparing nickel paste for barium titanate-based MLCC with reduced dielectric loss according to claim 6, Features: The organic and inorganic additives are added after being treated by the following method: The antimony pentoxide and the molten triphenyl antimony diacetate are mixed and dispersed uniformly, and the mixture is obtained by spray drying; the two molten materials, citrus stearic acid and lithium stearate, are mixed uniformly, sprayed onto the surface of the mixture, and cooled and dried; The added amounts of citric acid and lithium stearate are 2-5% and 4-8% of the mass of the mixture respectively.
8. The method for preparing nickel paste for barium titanate-based MLCC with reduced dielectric loss according to claim 6, Features: The stirring temperature in the glass reactor in step (1) is 80-90° C., and the melting temperature in the muffle furnace in step (2) is 1050-1300° C.
Citation Information
Patent Citations
A nickel internal electrode slurry with high dispersibility and low shrinkage and its preparation method
CN113948235B
Conductive paste for multilayer ceramic capacitor and preparation method thereof
CN101847510A
Cited By
Amorphous silicon oxide coated modified nickel powder electrode material for ceramic capacitor and preparation method of amorphous silicon oxide coated modified nickel powder electrode material
CN117583598A