A method for preparing phenolic epoxy fiber by dry spinning
Through the dry spinning method, phenols and aldehydes are produced in an acidic environment to generate high-ortho-position phenolic resin, which is mixed with epoxy resin for microwave curing. This solves the problems of deformation and environmental pollution in the thermal curing method of phenolic fibers and achieves The high mechanical properties and efficient curing of phenolic epoxy fiber are suitable for applications in many fields.
Patent Information
- Application Number
- CN202310684183.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-11
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-11
AI Technical Summary
Existing thermal curing methods for phenolic fibers have problems such as deformation, reduced mechanical properties, and environmental pollution. The solution curing efficiency is low, which affects the compactness and mechanical properties of the fibers.
Using dry spinning method, phenols and aldehydes are catalyzed by metal salts in an acidic environment to generate high-ortho-position phenolic resin, which is mixed with epoxy resin, and amine curing agent is added for microwave curing to form phenolic epoxy fiber. Environmental pollution and inefficient curing of hydrochloric acid-formaldehyde solution are avoided.
It improves the mechanical properties, heat resistance and curing efficiency of the fiber, reduces pollution, and has a uniform fiber structure, making it suitable for applications in many fields.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of heat-resistant, flame-retardant and insulating special fibers, and specifically relates to a method for preparing phenolic epoxy fibers by dry spinning. Background Art
[0002] Phenolic fiber is a flame-retardant fiber with a three-dimensional structure, which is obtained by polymerization, spinning and cross-linking of phenolic compounds and aldehyde compounds. Phenolic fiber has the advantages of heat resistance, flame retardancy, corrosion resistance, and good electrical insulation. It contains only three elements, C, H, and O. It produces very little smoke in the flame and no toxic gas. It can be used in the production of heat-resistant fabrics, friction materials, insulation materials, heat-resistant composite materials, etc. It can also be used in the fields of construction, aerospace, transportation, petrochemicals, etc.
[0003] At present, the main methods for cross-linking and curing phenolic fibers are thermal curing and solution curing. Pure thermoplastic phenolic fibers will deform after thermal curing. The small molecular water produced by thermosetting phenolic fibers during the thermal curing process will cause pores in the fibers, resulting in a decrease in mechanical properties. The commonly used curing agent is hexamethylenetetramine, but it will decompose when it exceeds 100°C, while the thermal curing temperature of phenolic fibers is mostly above 120°C, and the addition of curing agents will also affect the mechanical properties of the fibers. Therefore, the phenolic fiber system needs to be modified (Ji Kang, Lu Yutong, Wang Liuliu, Zhang Wei, Zhang Derong. Effect of curing agent on the performance of phenolic molding materials [J]. Engineering Plastics Application, 2021, 49(05): 137-142.). Solution curing usually uses hydrochloric acid-formaldehyde solution as the crosslinking bath. However, this curing method not only requires a long reaction time, but also hydrochloric acid and formaldehyde are both volatile substances, which will volatilize hydrochloric acid, formaldehyde and their compounds into the air, causing environmental pollution. The recovery and utilization of the hydrochloric acid-formaldehyde crosslinking bath is also a factor that needs to be considered (Wang Ying, Xie Gai, Liu Yong. Research Progress on Preparation of Phenolic Fibers by Electrospinning [J]. Polymer Bulletin, 2016(03):1-5.). Therefore, a curing method that can maintain the various properties of phenolic fiber, improve curing efficiency and protect the environment is needed.
[0004] Epoxy resin has excellent corrosion resistance, thermal stability, mechanical properties and heat resistance, and is widely used in electrical, electronic, optical, construction and other fields. The epoxy group in epoxy resin can react with the phenolic hydroxyl group and other groups in phenolic fiber, and under the action of amine curing agent, the system can be better cross-linked. Summary of the invention
[0005] The present invention provides a method for preparing phenolic epoxy fiber by dry spinning. After curing, the fiber morphology remains unchanged, the mechanical properties, heat resistance and curing efficiency are improved, the pollution is small and the efficiency is high. The prepared high-ortho-phenolic epoxy fiber has excellent flame retardancy and mechanical properties.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The present invention firstly reacts phenols and aldehydes in an acidic environment by metal salt catalysis to generate thermoplastic high-ortho-phenolic resin, mixes it with epoxy resin, adds amine curing agent to perform dry spinning, and performs microwave curing treatment on the obtained primary fiber to obtain flame-retardant and heat-resistant phenolic epoxy fiber prepared by dry spinning.
[0008] The present invention provides a method for preparing phenolic epoxy fiber by dry spinning, the steps of which are as follows:
[0009] (1) After mixing a phenolic compound, an aldehyde compound and a metal salt catalyst, the mixture is heated in a three-necked flask and kept in a boiling state for 4-4.5 hours, then an acidic catalyst is added and the reaction is continued for 1-1.5 hours, then the mixture is distilled under reduced pressure to 100-130° C., and then cooled to room temperature to obtain a high-ortho-phenolic resin;
[0010] (2) Mixing high-ortho-phenolic resin and epoxy resin, heating at 75-90°C to completely melt the resin to obtain high-ortho-phenolic / epoxy mixed resin, adding a small amount of organic solvent and heating to 92-97°C, adding an amine curing agent and stirring quickly, and then dry spinning to obtain phenolic epoxy primary fiber;
[0011] (3) The obtained primary fibers are subjected to microwave curing treatment to obtain phenolic epoxy fibers prepared by dry spinning.
[0012] The phenolic compound in step (1) is phenol, m-cresol or resorcinol; the aldehyde compound is formaldehyde or acetaldehyde; the metal salt catalyst is barium acetate; and the acid catalyst is hydrochloric acid, oxalic acid or sulfuric acid.
[0013] In the step (1), the molar ratio of the phenolic compound to the aldehyde compound is 1:(0.7-0.9); the mass ratio of the phenolic compound to the metal salt catalyst is 1:(0.01-0.025); and the mass ratio of the phenolic compound to the acidic catalyst is 1:(0.003-0.007).
[0014] During the vacuum distillation operation in step (1), the pressure in the device is 0.001-0.0017 MPa; and the heating rate during the vacuum distillation operation is 0.08-0.5°C / min.
[0015] The epoxy resin in step (2) is E-44, F-48 or F-704.
[0016] In the step (2), the amine curing agent is ethylenediamine, diethylenetriamine, diethylaminopropylamine, and the organic solvent is N,N-dimethylformamide, dimethyl sulfoxide or N,N-dimethylacetamide.
[0017] In the step (2), the mass ratio of high-ortho-phenolic resin to epoxy resin is 1:(0.05-2); the mass ratio of high-ortho-phenolic / epoxy mixed resin to organic solvent is 1:(0.01-0.5); and the mass ratio of high-ortho-phenolic / epoxy mixed resin to amine curing agent is 1:(0.005-0.025).
[0018] In the step (3), dry spinning is carried out in a nitrogen atmosphere at a tunnel temperature of 100-250° C. The obtained nascent fibers are placed in a microwave oven under air conditions and subjected to microwave treatment at a power of 60-1200 W for 1-30 min.
[0019] The beneficial effects of the present invention are:
[0020] The invention adopts a physical blending method to modify the thermoplastic phenolic resin, and obtains phenolic epoxy fiber by dry spinning. Compared with the existing modification method, the physical blending operation is simple, and the spinning can be performed only by mixing in proportion and heating the solution, thereby greatly improving the production efficiency. The epoxy group is used as a curing agent to reduce the release of small molecules in the reaction, improve the density of the fiber, and increase the mechanical properties of the fiber. The organic solvent used in the blending is conducive to the uniform mixing of the resin, and the obtained fiber structure is uniform. The microwave curing method is adopted to effectively avoid the environmental pollution caused by the hydrochloric acid-formaldehyde solution, the low curing efficiency and other problems. At the same time, the internal and external structures of the fiber are uniform, and the skin-core structure is eliminated. The phenolic epoxy fiber after microwave curing has the advantages of heat resistance, flame retardancy, strong toughness and the like, and can be applied to many fields such as construction, national defense, and transportation. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with specific embodiments. It should be understood that the following embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention, and those skilled in the art in this field can make some non-essential improvements and adjustments based on the content of the above invention. Example 1
[0022] This embodiment provides a method for preparing phenolic epoxy fiber by dry spinning, the steps are as follows:
[0023] (1) Phenol, formaldehyde and barium acetate were mixed and heated in an oil bath to keep them in a boiling state for 4 hours, and then sulfuric acid solution was added and the reaction was continued for 1 hour. Then, the mixture was placed in a vacuum distillation apparatus and heated to 100°C at a heating rate of 0.08°C / min, and the pressure in the apparatus was maintained at 0.001MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenol to formaldehyde was 1:0.7, the mass ratio of phenol to barium acetate was 1:0.01, and the mass ratio of phenol to sulfuric acid was 1:0.003.
[0024] (2) Mix high-ortho-phenolic resin and epoxy resin E-44, heat at 75°C to make the resin completely molten, and obtain high-ortho-phenolic / epoxy mixed resin. Add a small amount of dimethyl sulfoxide and stir well, then heat to 92°C, add ethylenediamine and stir quickly, then dry-spin in a nitrogen atmosphere at a tunnel temperature of 100°C to obtain phenolic epoxy primary fibers. The mass ratio of high-ortho-phenolic resin to epoxy resin is 1:0.05; the mass ratio of high-ortho-phenolic / epoxy mixed resin to dimethyl sulfoxide is 1:0.01; and the mass ratio of high-ortho-phenolic / epoxy mixed resin to ethylenediamine is 1:0.005.
[0025] (3) The obtained spun fibers were cured by microwave at a power of 60 W for 30 min in a nitrogen atmosphere at a temperature of 100 °C to obtain phenolic epoxy fibers prepared by dry spinning.
[0026] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 35, the elongation at break is 74%, the strength is 8.2 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 50%, the modulus is 36 cN / dtex, and the thermal decomposition temperature in nitrogen is 343°C. Example 2
[0027] This embodiment provides a method for preparing phenolic epoxy fiber by dry spinning, the steps are as follows:
[0028] (1) After m-cresol is mixed with acetaldehyde and barium acetate, it is heated in an oil bath to keep it in a boiling state for 4.5 hours, and then hydrochloric acid solution is added, and the reaction is continued for 1.5 hours, and then it is placed in a vacuum distillation device and heated to 130°C at a heating rate of 0.5°C / min, and the pressure in the device is maintained at 0.0017MPa. When the solution is in a viscous state that can be drawn into threads, it is poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenol: aldehyde compound is 1:0.9; the mass ratio of phenol compound: barium acetate is 1:0.025; and the mass ratio of phenol compound to acid catalyst is 1:0.007.
[0029] (2) Mix high-ortho-phenolic resin and epoxy resin F-48, heat at 90°C to make the resin completely molten, and obtain high-ortho-phenolic / epoxy mixed resin. Add a small amount of N,N-dimethylformamide and stir well. Heat to 97°C, add diethylenetriamine and stir quickly. Then dry-spin in a nitrogen atmosphere at a tunnel temperature of 250°C to obtain phenolic epoxy primary fibers. The mass ratio of high-ortho-phenolic resin to epoxy resin is 1:2; the mass ratio of high-ortho-phenolic / epoxy mixed resin to N,N-dimethylformamide is 1:0.5; and the mass ratio of high-ortho-phenolic / epoxy mixed resin to diethylenetriamine is 1:0.025.
[0030] (3) The obtained spun fibers were microwave cured for 1 min at a power of 1200 W in a nitrogen atmosphere at a temperature of 250°C to obtain phenolic epoxy fibers prepared by dry spinning.
[0031] According to the test results, the phenolic fiber obtained has a limiting oxygen index of 33, an elongation at break of 74%, a strength of 6.2 cN / dtex, a residual carbon rate of 49% under a nitrogen atmosphere of 900°C, a modulus of 34 cN / dtex, and a thermal decomposition temperature of 373°C in nitrogen. Example 3
[0032] This embodiment provides a method for preparing phenolic epoxy fiber by dry spinning, the steps are as follows:
[0033] (1) Resorcinol was mixed with formaldehyde and barium acetate and heated in an oil bath to keep it in a boiling state for 4.2 hours, and then hydrochloric acid solution was added and the reaction was continued for 1.5 hours. Then it was placed in a vacuum distillation device and heated to 120°C at a heating rate of 0.4°C / min, and the pressure in the device was maintained at 0.0015MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenolic compound to aldehyde compound was 1:0.8; the mass ratio of phenolic compound to barium acetate was 1:0.02; and the mass ratio of phenolic compound to acidic catalyst was 1:0.004.
[0034] (2) Mix high-ortho-phenolic resin and epoxy resin F-704, heat at 80°C to make the resin completely molten, and obtain high-ortho-phenolic / epoxy mixed resin. Add a small amount of N,N-dimethylacetamide and stir well, then heat to 95°C, add diethylaminopropylamine and stir quickly, and then dry-spin in a nitrogen atmosphere at a channel temperature of 150°C to obtain phenolic epoxy primary fibers. The mass ratio of high-ortho-phenolic resin to epoxy resin is 1:1; the mass ratio of high-ortho-phenolic / epoxy mixed resin to N,N-dimethylacetamide is 1:0.1; and the mass ratio of high-ortho-phenolic / epoxy mixed resin to diethylaminopropylamine is 1:0.02.
[0035] (3) The obtained spun fibers were cured by microwave at a power of 1000 W for 4 min in a nitrogen atmosphere at a temperature of 100-250° C. to obtain phenolic epoxy fibers prepared by dry spinning.
[0036] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 35, the elongation at break is 84%, the strength is 7.2 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 59%, the modulus is 34 cN / dtex, and the thermal decomposition temperature in nitrogen is 393°C. Example 4
[0037] This embodiment provides a method for preparing phenolic epoxy fiber by dry spinning, the steps are as follows:
[0038] (1) Phenol, formaldehyde and barium acetate were mixed and heated in an oil bath to keep them in a boiling state for 4.2 hours, and then hydrochloric acid solution was added and the reaction was continued for 1.5 hours. Then, the mixture was placed in a vacuum distillation apparatus and heated to 120°C at a heating rate of 0.4°C / min, and the pressure in the apparatus was maintained at 0.0015MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenolic compound to aldehyde compound was 1:0.85, the mass ratio of phenolic compound to barium acetate was 1:0.02, and the mass ratio of phenolic compound to acidic catalyst was 1:0.004.
[0039] (2) Mix high-ortho-phenolic resin and epoxy resin F-704, heat at 80°C to make the resin completely molten, and obtain high-ortho-phenolic / epoxy mixed resin. Add a small amount of N,N-dimethylacetamide and stir well. Heat to 95°C, add diethylaminopropylamine and stir quickly. Then dry-spin in a nitrogen atmosphere at a tunnel temperature of 180°C to obtain phenolic epoxy primary fibers. The mass ratio of high-ortho-phenolic resin to epoxy resin is 1:1; the mass ratio of high-ortho-phenolic / epoxy mixed resin to N,N-dimethylacetamide is 1:0.1; and the mass ratio of high-ortho-phenolic / epoxy mixed resin to diethylaminopropylamine is 1:0.02.
[0040] (3) The obtained spun fibers were cured by microwave at a power of 800 W for 7 min in a nitrogen atmosphere at a tunnel temperature of 150°C to obtain phenolic epoxy fibers prepared by dry spinning.
[0041] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 35, the elongation at break is 74%, the strength is 3.2 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 39%, the modulus is 24 cN / dtex, and the thermal decomposition temperature in nitrogen is 381°C. Example 5
[0042] This embodiment provides a method for preparing phenolic epoxy fiber by dry spinning, the steps are as follows:
[0043] (1) Phenol, formaldehyde and barium acetate were mixed and heated in an oil bath to keep them in a boiling state for 4 hours, and then sulfuric acid solution was added and the reaction was continued for 1 hour. Then, the mixture was placed in a vacuum distillation apparatus and heated to 100°C at a heating rate of 0.08°C / min, and the pressure in the apparatus was maintained at 0.001MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenol to formaldehyde was 1:0.85, the mass ratio of phenol to barium acetate was 1:0.01, and the mass ratio of phenol to sulfuric acid was 1:0.003.
[0044] (2) Mix high-ortho-phenolic resin and epoxy resin E-44, heat at 75°C to make the resin completely molten, and obtain high-ortho-phenolic / epoxy mixed resin. Add a small amount of dimethyl sulfoxide and stir well, heat to 92°C, add ethylenediamine and stir quickly, and then dry-spin in a nitrogen atmosphere at a tunnel temperature of 240°C to obtain phenolic epoxy primary fibers. The mass ratio of high-ortho-phenolic resin to epoxy resin is 1:0.05; the mass ratio of high-ortho-phenolic / epoxy mixed resin to dimethyl sulfoxide is 1:0.01; and the mass ratio of high-ortho-phenolic / epoxy mixed resin to ethylenediamine is 1:0.005.
[0045] (3) The obtained spun fibers were microwave cured for 10 min at a temperature of 180°C and a power of 600 W in a nitrogen atmosphere to obtain phenolic epoxy fibers prepared by dry spinning.
[0046] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 35, the elongation at break is 89%, the strength is 4.2 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 50%, the modulus is 36 cN / dtex, and the thermal decomposition temperature in nitrogen is 343°C. Example 6
[0047] This embodiment provides a method for preparing phenolic epoxy fiber by dry spinning, the steps are as follows:
[0048] (1) After m-cresol is mixed with acetaldehyde and barium acetate, it is heated in an oil bath to keep it in a boiling state for 4.5 hours, and then hydrochloric acid solution is added, and the reaction is continued for 1.5 hours, and then it is placed in a vacuum distillation device and heated to 130°C at a heating rate of 0.5°C / min, and the pressure in the device is maintained at 0.0017MPa. When the solution is in a viscous state that can be drawn into threads, it is poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenolic compound: aldehyde compound is 1:0.85, the mass ratio of phenolic compound: barium acetate is 1:0.025; the mass ratio of phenolic compound to acidic catalyst is 1:0.007.
[0049] (2) Mix high-ortho-phenolic resin and epoxy resin F-48, heat at 90°C to make the resin completely molten, and obtain high-ortho-phenolic / epoxy mixed resin. Add a small amount of N,N-dimethylformamide and stir well, then heat to 97°C, add diethylenetriamine and stir quickly, and then dry-spin in a nitrogen atmosphere at a tunnel temperature of 140°C to obtain phenolic epoxy primary fibers. The mass ratio of high-ortho-phenolic resin to epoxy resin is 1:2; the mass ratio of high-ortho-phenolic / epoxy mixed resin to N,N-dimethylformamide is 1:0.5; and the mass ratio of high-ortho-phenolic / epoxy mixed resin to diethylenetriamine is 1:0.025.
[0050] (3) The obtained spun fibers were cured by microwave in a nitrogen atmosphere at a temperature of 210°C and a power of 1000 W for 10 min to obtain phenolic epoxy fibers prepared by dry spinning.
[0051] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 37, the elongation at break is 73%, the strength is 4.2 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 49%, the modulus is 34 cN / dtex, and the thermal decomposition temperature in nitrogen is 393°C. Example 7
[0052] This embodiment provides a method for preparing phenolic epoxy fiber by dry spinning, the steps are as follows:
[0053] (1) Resorcinol was mixed with formaldehyde and barium acetate and heated in an oil bath to keep it in a boiling state for 4.2 hours, and then hydrochloric acid solution was added and the reaction was continued for 1.5 hours. Then it was placed in a vacuum distillation device and heated to 120°C at a heating rate of 0.4°C / min, and the pressure in the device was maintained at 0.0015MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenolic compound to aldehyde compound was 1:0.88, the mass ratio of phenolic compound to barium acetate was 1:0.02, and the mass ratio of phenolic compound to acidic catalyst was 1:0.004.
[0054] (2) Mix high-ortho-phenolic resin and epoxy resin F-704, heat at 80°C to make the resin completely molten, and obtain high-ortho-phenolic / epoxy mixed resin. Add a small amount of N,N-dimethylacetamide and stir well, then heat to 95°C, add diethylaminopropylamine and stir quickly, and then dry-spin in a nitrogen atmosphere at a tunnel temperature of 110°C to obtain phenolic epoxy primary fibers. The mass ratio of high-ortho-phenolic resin to epoxy resin is 1:1; the mass ratio of high-ortho-phenolic / epoxy mixed resin to N,N-dimethylacetamide is 1:0.1; and the mass ratio of high-ortho-phenolic / epoxy mixed resin to diethylaminopropylamine is 1:0.02.
[0055] (3) The obtained spun fibers were microwave cured for 6 min at a temperature of 200°C and a power of 800 W in a nitrogen atmosphere to obtain phenolic epoxy fibers prepared by dry spinning.
[0056] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 35, the elongation at break is 34%, the strength is 9.2 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 59%, the modulus is 34 cN / dtex, and the thermal decomposition temperature in nitrogen is 313°C. Example 8
[0057] This embodiment provides a method for preparing phenolic epoxy fiber by dry spinning, the steps are as follows:
[0058] (1) Phenol, formaldehyde and barium acetate were mixed and heated in an oil bath to keep them in a boiling state for 4.2 hours, and then hydrochloric acid solution was added and the reaction was continued for 1.5 hours. Then, the mixture was placed in a vacuum distillation apparatus and heated to 120°C at a heating rate of 0.3°C / min, and the pressure in the apparatus was maintained at 0.0015MPa. When the solution was in a viscous state that could be drawn into threads, it was poured out and cooled to room temperature to obtain a high-ortho-phenolic resin. The molar ratio of phenolic compound to aldehyde compound was 1:0.82, the mass ratio of phenolic compound to barium acetate was 1:0.02, and the mass ratio of phenolic compound to acidic catalyst was 1:0.004.
[0059] (2) Mix high-ortho-phenolic resin and epoxy resin F-704, heat at 80°C to make the resin completely molten, and obtain high-ortho-phenolic / epoxy mixed resin. Add a small amount of N,N-dimethylacetamide and stir well, then heat to 95°C, add diethylaminopropylamine and stir quickly, and then dry-spin in a nitrogen atmosphere at a channel temperature of 190°C to obtain phenolic epoxy primary fibers. The mass ratio of high-ortho-phenolic resin to epoxy resin is 1:1; the mass ratio of high-ortho-phenolic / epoxy mixed resin to N,N-dimethylacetamide is 1:0.1; and the mass ratio of high-ortho-phenolic / epoxy mixed resin to diethylaminopropylamine is 1:0.02.
[0060] (3) The obtained spun fibers were microwave cured for 4 min at a temperature of 240°C in a nitrogen atmosphere at a power of 900 W to obtain phenolic epoxy fibers prepared by dry spinning.
[0061] According to the test results, the limiting oxygen index of the phenolic fiber obtained is 33, the elongation at break is 94%, the strength is 3.2 cN / dtex, the residual carbon rate under 900°C nitrogen atmosphere is 39%, the modulus is 24 cN / dtex, and the thermal decomposition temperature in nitrogen is 382°C.
[0062] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A method for preparing phenolic epoxy fiber by dry spinning, characterized in that Here are the steps: (1) After mixing a phenolic compound, an aldehyde compound and a metal salt catalyst, the mixture is heated in a three-necked flask and kept in a boiling state for 4-4.5 hours, an acidic catalyst is added and the reaction is continued for 1-1.5 hours, and then the mixture is distilled under reduced pressure to 100-130° C. and cooled to room temperature to obtain a high-ortho-phenolic resin; (2) Mixing high-ortho-phenolic resin and epoxy resin, heating at 75-90°C to completely melt the resin to obtain high-ortho-phenolic / epoxy mixed resin; adding a small amount of organic solvent and heating to 92-97°C, adding an amine curing agent and stirring quickly, and then dry spinning to obtain phenolic epoxy primary fiber; (3) The obtained primary fibers are subjected to microwave curing treatment to obtain phenolic epoxy fibers prepared by dry spinning; In step (2), the epoxy resin is E-44, F-48 or F-704; In the step (2), the mass ratio of high-ortho-phenolic resin to epoxy resin is 1:(0.05-2); the mass ratio of high-ortho-phenolic / epoxy mixed resin to organic solvent is 1:(0.01-0.5); and the mass ratio of high-ortho-phenolic / epoxy mixed resin to amine curing agent is 1:(0.005-0.025).
2. The method for preparing phenolic epoxy fiber by dry spinning according to claim 1, characterized in that: The phenolic compound in step (1) is phenol, m-cresol or resorcinol; the aldehyde compound is formaldehyde or acetaldehyde; the metal salt catalyst is barium acetate; and the acid catalyst is hydrochloric acid, oxalic acid or sulfuric acid.
3. The method for preparing phenolic epoxy fiber by dry spinning according to claim 1, characterized in that: In the step (1), the molar ratio of the phenolic compound to the aldehyde compound is 1:(0.7-0.9); the mass ratio of the phenolic compound to the metal salt catalyst is 1:(0.01-0.025); and the mass ratio of the phenolic compound to the acidic catalyst is 1:(0.003-0.007).
4. The method for preparing phenolic epoxy fiber by dry spinning according to claim 1, characterized in that: During the vacuum distillation operation in step (1), the pressure in the device is 0.001-0.0017 MPa; and the heating rate during the vacuum distillation operation is 0.08-0.5°C / min.
5. The method for preparing phenolic epoxy fiber by dry spinning according to claim 1, characterized in that: In the step (2), the amine curing agent is ethylenediamine, diethylenetriamine, diethylaminopropylamine, and the organic solvent is N,N-dimethylformamide, dimethyl sulfoxide or N,N-dimethylacetamide.
6. The method for preparing phenolic epoxy fiber by dry spinning according to claim 1, characterized in that: In the step (3), dry spinning is carried out in a nitrogen atmosphere at a tunnel temperature of 100-250° C. The obtained nascent fibers are placed in a microwave oven under air conditions and subjected to microwave treatment at a power of 60-1200 W for 1-30 min.
Citation Information
Patent Citations
Epoxy-phenol-formaldehyde resin prepreg and preparation method therefor
CN106167599A
Method for preparing high-ortho thermosetting phenol-formaldehyde fibers by wet spinning
CN109208116A