A Cu2O / Cu heterostructure nanomaterial synthesized by thermal decomposition and its preparation method and application

The Cu2O/Cu heterostructure nanomaterials are synthesized by thermal decomposition method, which solves the problems of high cost and complicated operation in the existing technology, and realizes the dual properties of nanomaterials and efficient photocatalytic CO2 reduction reaction.

CN116651453BActive Publication Date: 2024-10-15NANJING TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310631479.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-10-15
Estimated Expiration
2043-05-31

AI Technical Summary

Technical Problem

Existing methods for synthesizing Cu2O/Cu nanoheterostructures have problems such as high cost, complex operations, and long time consumption, making it difficult to effectively optimize the performance of a single metal or a single oxide.

Method used

Using the thermal decomposition method, the oxygen-containing copper precursor is mixed with an organic solvent, and after heating and cooling, a Cu2O/Cu heterostructure nanomaterial is formed, and a photocatalytic CO2 reduction reaction is performed in a vacuum state.

Benefits of technology

A low-cost, simple-to-operate synthesis of Cu2O/Cu heterostructure nanomaterials is achieved. It has the dual properties of oxide and metal element, optimizes the catalytic performance, and shows high efficiency in the photocatalytic CO2 reduction reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116651453B_ABST
    Figure CN116651453B_ABST
Patent Text Reader

Abstract

The present invention discloses a Cu2O / Cu heterostructure nanomaterial synthesized by thermal decomposition, and a preparation method and application thereof. The formation of the structure utilizes the Kirkendall effect. Since the Cu2O surface is reduced to Cu, the different diffusion rates of oxygen atoms inside and outside the particles eventually lead to the formation of a nano heterostructure. The method of the present invention is simple to operate and low in cost. The synthesized oxide / metal nano heterostructure material can have the properties of oxide and metal element at the same time. The metal nanostructure capped with oxide has multifunctionality and synergistic effect, and can have the properties of two substances at the same time. Under the interaction of these two properties, the structure can be applied to catalysis, photonics, and other wider fields to produce more excellent effects. The performance of a single metal or a single oxide can be optimized, and it is expected to explore more potential properties of the composite structure and apply it to a wider range of fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of synthesis of nano metals and their oxides, and specifically relates to a Cu 2 O / Cu heterostructure nanomaterials and their preparation methods and applications. Background Art

[0002] Cuprous oxide (Cu 2 Copper (Cu) is a stable copper oxide. Because it behaves like a P-type semiconductor and has a theoretical direct band gap of 2.2 eV, it is highly active and selective for many oxidation / reduction reactions and is one of the most commonly used catalysts. In addition, it is also an important component in materials such as high-temperature superconductors, biosensors, medicine, water decomposition, and environmental pollutants. Copper (Cu) is a very important metal material. Due to its good ductility, conductivity and low cost, it is an important material for industrial production and can be used in electrical conduction, thermal conduction, catalysis, medicine, energy, machinery manufacturing, national defense and other fields. At the nanoscale, the material has macroscopic quantum tunneling effect, small size effect, surface effect, Gibbs-Thomson effect, etc., so nanomaterials will show more superior performance than bulk materials.

[0003] Currently synthesized Cu 2 The methods for preparing O / Cu nano heterostructures include chemical reduction and magnetron sputtering. The chemical reduction method uses a wide variety of chemicals, a complex reaction process and takes a long time, and the magnetron sputtering equipment system is complex and expensive. The raw materials, principles and processes used in the thermal decomposition method used in the present invention are relatively simple, and the most basic chemical device can be used to quickly obtain the product. Summary of the invention

[0004] Purpose of the invention: The technical problem to be solved by the present invention is to provide a low-cost, simple-to-operate Cu 2 O / Cu heterostructure nanomaterials and their synthesis methods achieve the properties of both oxides and metal elements, further optimizing the performance of single metals or single oxides.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A Cu synthesized by thermal decomposition 2 The method for O / Cu heterostructure nanomaterials comprises the following steps:

[0007] (1) mixing a copper precursor containing oxygen and an organic solvent, and fully stirring at 25 to 80° C. to form a uniform suspension;

[0008] (2) The suspension of step (1) is heated to 100-350° C. in an inert gas atmosphere, kept warm for 5-360 min, then cooled to room temperature, centrifuged, dried, and ground to obtain the product.

[0009] Specifically, in step (1), the copper precursor containing oxygen element is selected from any one or a combination of two or more of basic copper carbonate, basic copper acetate, basic copper nitrate, basic copper nitrite, anhydrous copper acetate, cuprous acetate, copper formate, copper hydroxide, copper oxalate, and copper oxide; the organic solvent is selected from any one or a combination of two or more of olefins or alkynes containing more than 12 carbon atoms and their isomers, preferably octadecene, hexadecene or octadecene.

[0010] Specifically, in step (1), the copper precursor containing oxygen element and the organic solvent are mixed in a mass ratio of 1:(4-12), and the mixing is carried out by magnetic stirring or mechanical stirring at a stirring speed of 50-700 r / min for 10-30 min.

[0011] Preferably, in step (2), the inert gas is nitrogen or argon.

[0012] Preferably, in step (2), the centrifugal speed is 6000-10000 r / min; the centrifugal time is 5-20 min; the detergent used for centrifugation is a mixture of n-hexane and ethanol, preferably in a volume ratio of 3:1.

[0013] Preferably, in step (2), the drying temperature is 60 to 80° C., and the drying time is 30 to 120 min.

[0014] Furthermore, the Cu prepared by the above preparation method 2 O / Cu heterostructure nanomaterials are also within the protection scope of the present invention.

[0015] Furthermore, the present invention also claims the above-mentioned Cu 2 O / Cu heterostructure nanomaterials for photocatalytic CO 2 Restore the app.

[0016] Specifically, the present invention converts the above-mentioned Cu 2 O / Cu heterostructure nanomaterials for photocatalytic CO 2 The restoration process includes the following steps:

[0017] S1: Cu 2 The O / Cu heterostructure nanomaterials were placed in a reaction vessel and darkly adsorbed under vacuum for 6 to 24 h;

[0018] S2: Introduce the CO to be reduced into the reaction vessel 2and inject deionized water, and under the irradiation of light, the Cu 2 O / Cu heterostructure nanomaterials as photocatalysts for CO 2 The gas undergoes a photocatalytic reduction reaction.

[0019] Specifically, in step S2, the high-purity CO 2 The concentration of the photocatalyst is 99.999%; 2 The mass ratio of the photocatalyst to deionized water is 1:(0.5-2).

[0020] Specifically, in step S2, the light source is any one of a xenon lamp, an LED lamp, a mercury lamp, a UVC lamp, a metal halide lamp or a solar simulator, or a mixture of two or more thereof.

[0021] Beneficial effects:

[0022] (1) The present invention synthesizes cuprous oxide / copper nanostructures by liquid phase high temperature thermal decomposition. The formation of the structure utilizes the Kirkendall effect. 2 The surface of O is reduced to Cu, and the different diffusion rates of oxygen atoms inside and outside the particles eventually lead to the formation of nano heterogeneous structures. When selecting raw materials, considering the need to retain the components of metal oxides, the present invention uses copper salts containing oxygen atoms and easily decomposed by heat to generate copper oxides as precursors, and selects organic solvents with weak reducing properties that do not coordinate with copper ions as reducing agents.

[0023] (2) The present invention uses a low-cost, simple-to-operate method to synthesize oxide / metal nanoheterostructure nanomaterials. The structure can have the properties of both oxide and metal. The metal nanostructure capped with oxide has multifunctionality and synergistic effects, and can have the properties of two substances at the same time. Under the interaction of these two properties, the structure can be applied to catalysis, photonics, and other wider fields, producing more excellent effects. The performance of a single metal or a single oxide can be optimized, and it is expected to explore more potential properties of the composite structure and apply it to a wider range of fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0025] Figure 1 It is a schematic flow diagram of the thermal decomposition reaction of the present invention.

[0026] Figure 2 is the XRD of the product in Example 1.

[0027] Figure 3 This is the SEM image of the product in Example 1.

[0028] Figure 4 is the particle size distribution of the product in Example 1.

[0029] Figure 5 This is a TEM image of the product in Example 1.

[0030] Figure 6 This is a schematic diagram of the photocatalytic effect in Example 1.

[0031] Figure 7 This is the XRD of the product in Comparative Example 1. DETAILED DESCRIPTION

[0032] The present invention can be better understood with reference to the following examples.

[0033] Example 1

[0034] The present invention adopts Figure 1 The Cu synthesized by thermal decomposition is shown in the process 2 O / Cu heterostructure nanomaterials specifically include the following steps:

[0035] (1) 10 mmol of basic copper carbonate and 30 ml of octadecene were mixed in a four-necked flask, heated to 80°C under magnetic stirring (400 r / min), and kept warm for 20 min. The mixture was then heated to 300°C in a nitrogen atmosphere (0.2 L / min), kept at this temperature for 1 hour, and then cooled to room temperature.

[0036] (2) The reaction solution was centrifuged using a mixed solution of n-hexane and ethanol in a ratio of 3:1 at 8000 r / min for 5 minutes. This operation was repeated until the upper layer was clear and transparent. The product was then placed in an oven at 80°C and dried for 30 minutes. The XRD pattern of the obtained product is shown in FIG. Figure 2 As shown, the phase composition of the product is cuprous oxide and copper. The diffraction peak of copper is stronger and cuprous oxide is weaker. The SEM results are as follows Figure 3 As shown, the obtained product is spherical particles with uniform morphology. The particles are relatively dispersed without agglomeration. The powder particle size distribution is as follows Figure 4 As shown in Figure 1, the average particle size is 40 nm. Figure 5 As shown, it can be clearly observed that the outer surface of the copper particles is covered with an amorphous oxide layer with a lattice spacing of Corresponding to the cuprous oxide (111) crystal plane.

[0037] (3) Take 500 mg of the Cu synthesized above 2 O / Cu heterostructure nanomaterials were placed at 15.4 cm 3In the photocatalytic device, the device was kept in a vacuum state, and after dark adsorption for 12 hours, high-purity CO was introduced. 2 When atmospheric pressure reached, 1 ml of deionized water was injected into the device, and the photocatalytic reaction was carried out under the irradiation of a xenon lamp. The CO / CH 4 The content of Figure 6 As shown, the structure is photocatalytic CO 2 The reduction experiment showed 0.029588μmol·(g·min) -1 The CO release rate and 0.025034 μmol·(g·min) -1 CH 4 Release rate.

[0038] Example 2

[0039] (1) 10 mmol of anhydrous copper acetate and 30 ml of octadecene were mixed and placed in a four-necked flask, heated to 80°C under magnetic stirring (400 r / min) and kept warm for 20 min. The mixture was then heated to 300°C in a nitrogen atmosphere (0.2 L / min), kept at this temperature for 1 hour, and then cooled to room temperature.

[0040] (2) The reaction solution was centrifuged using a mixed solution of n-hexane and ethanol in a ratio of 3:1 at 8000 r / min for 5 minutes. This operation was repeated until the upper liquid was clear and transparent. The product was then placed in an oven at 80° C. and dried for 30 minutes.

[0041] (3) Take 500 mg of the Cu synthesized above 2 O / Cu heterostructure nanomaterials were placed at 15.4 cm 3 In the photocatalytic device, the device was kept in a vacuum state, and after dark adsorption for 12 hours, high-purity CO was introduced. 2 When atmospheric pressure reaches 1 ml, 1 ml of deionized water is injected into the device. The photocatalytic reaction is carried out under the irradiation of a xenon lamp. The CO / CH 4 The structure is photocatalytic CO 2 The reduction experiment showed 0.019557μmol·(g·min) -1 The CO release rate and 0.011126667μmol·(g·min) -1 CH 4 Release rate.

[0042] Example 3

[0043] (1) 10 mmol of copper oxide and 30 ml of octadecene were mixed in a four-necked flask, heated to 80°C under magnetic stirring (400 r / min), and kept warm for 20 min. The mixture was then heated to 280°C in a nitrogen atmosphere (0.2 L / min), kept at this temperature for 1 hour, and then cooled to room temperature.

[0044] (2) The reaction solution was centrifuged using a mixed solution of n-hexane and ethanol in a ratio of 3:1 at 8000 r / min for 5 minutes. This operation was repeated until the upper liquid was clear and transparent. The product was then placed in an oven at 80° C. and dried for 1 hour.

[0045] (3) Take 500 mg of the Cu synthesized above 2 O / Cu heterostructure nanomaterials were placed at 15.4 cm 3 In the photocatalytic device, the device was kept in a vacuum state, and after dark adsorption for 12 hours, high-purity CO was introduced. 2 When atmospheric pressure reached, 1 ml of deionized water was injected into the device, and the photocatalytic reaction was carried out under the irradiation of a xenon lamp. The CO / CH 4 The structure is photocatalytic CO 2 The reduction experiment showed 0.044229667μmol·(g·min) -1 The CO release rate and 0.124696333 μmol·(g·min) -1 CH 4 Release rate.

[0046] Comparative Example 1

[0047] (1) 10 mmol of basic copper carbonate and 30 ml of octadecene were mixed and placed in a four-necked flask, heated to 80°C under magnetic stirring (400 r / min) and kept warm for 20 min. The mixture was then heated to 200°C in a nitrogen atmosphere (0.2 L / min), kept at this temperature for 1 hour, and then cooled to room temperature.

[0048] (2) The reaction solution was centrifuged using a mixed solution of n-hexane and ethanol in a ratio of 3:1 at 8000 r / min for 5 minutes. This operation was repeated until the upper layer was clear and transparent. The product was then placed in an oven at 80°C and dried for 1 hour. The XRD pattern of the obtained powder is shown in FIG. Figure 7 At this temperature, basic copper carbonate is gradually reduced to cuprous oxide, and no copper is generated, so the cuprous oxide / copper heterostructure cannot be synthesized.

[0049] The present invention provides a Cu synthesized by thermal decomposition 2The ideas and methods of O / Cu heterostructure nanomaterials and their preparation methods and applications, and the specific methods and approaches to realize the technical solution are many. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the protection scope of the present invention. All components not specified in this embodiment can be implemented by existing technologies.

Claims

1. A method for synthesizing Cu2O / Cu heterostructure nanomaterials by thermal decomposition, characterized in that: The steps include: (1) Mixing a copper precursor containing oxygen and an organic solvent, and stirring them thoroughly at 25-80 °C to form a uniform suspension; (2) heating the suspension of step (1) to 280-350°C in an inert atmosphere, keeping the temperature for 5-360 min, then cooling to room temperature, centrifuging, drying and grinding to obtain the product; In step (1), the copper precursor containing oxygen is selected from basic copper carbonate; the organic solvent is octadecene; In step (1), the copper precursor containing oxygen element and the organic solvent are mixed in a mass ratio of 1:(4-12), and the mixing is carried out by magnetic stirring or mechanical stirring at a stirring speed of 50-700 r / min for 10-30 min; The nano material is a Cu2O layer wrapped around the outer surface of a Cu particle.

2. The method for synthesizing Cu2O / Cu heterostructure nanomaterials by thermal decomposition according to claim 1, characterized in that: In step (2), the inert atmosphere is nitrogen or argon.

3. The method for synthesizing Cu2O / Cu heterostructure nanomaterials by thermal decomposition according to claim 1, characterized in that: In step (2), the centrifugal speed is 6000-10000 r / min; the centrifugal time is 5-20 min; and the detergent used for centrifugation is a mixture of n-hexane and ethanol.

4. The method for synthesizing Cu2O / Cu heterostructure nanomaterials by thermal decomposition according to claim 1, characterized in that: In step (2), the drying temperature is 60-80°C and the drying time is 30-120 min.

5. The Cu2O / Cu heterostructure nanomaterial prepared by the method according to any one of claims 1 to 4.

6. Use of the Cu2O / Cu heterostructure nanomaterial according to claim 5 for photocatalytic CO2 reduction.

7. The use according to claim 6, characterized in that: The steps include: S1: Place the Cu2O / Cu heterostructure nanomaterials in a reaction vessel and perform dark adsorption under vacuum for 6-24 h; S2: CO2 to be reduced is introduced into the reaction container and deionized water is injected. Under the irradiation of the light source, the Cu2O / Cu heterostructure nanomaterial acts as a photocatalyst to perform a photocatalytic reduction reaction on the CO2 gas.

8. The use according to claim 7, characterized in that: In step S2, the mass ratio of the photocatalyst to CO2 is 1:(0.5~2); the mass ratio of the photocatalyst to deionized water is 1:(0.5~2); the light source is any one of a xenon lamp, an LED lamp, a mercury lamp, a UVC lamp, a metal halide lamp or a solar simulator, or a mixture of two or more thereof.