A method for preparing melamine formaldehyde resin aerogel by drying at normal pressure

By introducing water-soluble polymer materials into melamine-formaldehyde resin as a template, the sol-gel method is used to prepare melamine-formaldehyde resin aerogels, which solves the problem of normal pressure drying preparation and achieves efficient and low-cost aerogel production with excellent Excellent mechanical properties and flame retardant properties, suitable for a variety of applications.

CN116655998BActive Publication Date: 2024-10-01XIHUA UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310669008.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-07
Publication Date
2024-10-01
Estimated Expiration
2043-06-07

AI Technical Summary

Technical Problem

It is difficult to prepare melamine formaldehyde resin aerogel materials with excellent mechanical properties and flame retardant properties through normal pressure drying using existing technology, and traditional drying processes are expensive and difficult to achieve large-scale production.

Method used

Using hydroxymethylated melamine and water-soluble polymer materials as templates, the melamine-formaldehyde resin hydrogel is grown through in-situ condensation by the sol-gel method, and the aerogel is produced by drying under normal pressure. The polymer material is used to enhance the gel's strength. Toughness and strength, resisting the effects of surface tension.

Benefits of technology

Achieved the preparation of melamine formaldehyde resin aerogels with low density, high porosity and moderate thermal conductivity without using solvent exchange. It has excellent thermal insulation and flame retardant properties and is suitable for flame retardant, thermal insulation and fireproof materials. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116655998B_ABST
    Figure CN116655998B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing melamine formaldehyde resin aerogel by drying at normal pressure, which belongs to the field of polymer materials. The method comprises preparing hydrogel from hydroxymethylated melamine and polymer template by sol-gel method, and then preparing aerogel from the obtained hydrogel by drying at normal pressure; wherein the mass ratio of hydroxymethylated melamine to polymer template is 3 to 10:1, and the pH value is adjusted to 1 to 6 in the sol-gel method. The preparation method of the present invention does not adopt any solvent replacement, and the aerogel material can be obtained by directly drying the hydrogel, which is simple to operate, low in cost, good in environmental benefits, and good in economic benefits. The melamine formaldehyde resin aerogel obtained by the present invention has a dense structure, a relatively low pore size, excellent thermal insulation performance, and intrinsic flame retardant performance, and has the potential to be applied to flame retardant materials, thermal insulation materials, fireproof materials, and buffer materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing melamine formaldehyde resin aerogel by drying at normal pressure, and belongs to the field of polymer materials. Background Art

[0002] As the problem of global warming becomes increasingly serious, energy conservation and emission reduction has become a hot topic in society. The use of thermal insulation materials is one of the most direct and effective ways to save energy and reduce emissions. At present, the most commonly used thermal insulation material is rigid polyurethane foam. However, its flammable nature makes it have a high fire hazard. Flame retardant modification of rigid polyurethane foam can effectively improve the flame retardant properties of the foam, but the addition of flame retardants will destroy the microstructure of the foam material, which will lead to a decrease in the thermal insulation performance of the material. Aerogel is considered to be an ideal substitute for traditional thermal insulation materials due to its advantages such as high porosity, low density, low thermal conductivity and excellent mechanical properties. However, the preparation of aerogels often requires special drying processes to reduce the collapse of the pore structure and large-scale shrinkage caused by the surface tension of the solvent, which in turn leads to damage to the thermal insulation and mechanical properties of the material. These special drying processes are supercritical drying and freeze drying, which are expensive and difficult to achieve large-scale and continuous production of aerogels, thus hindering the widespread application of aerogels.

[0003] Drying at normal pressure is considered to be an ideal method for large-scale aerogel production. At present, the methods for achieving normal pressure drying of aerogels are to increase the pore size, enhance the strength of the aerogel skeleton, and use low surface tension for solvent replacement. Aerogels have disadvantages such as cumbersome preparation process and the use of a large amount of toxic and harmful organic solvents. At present, there are many studies on normal pressure drying of silica aerogel materials, and the methods are relatively mature. However, inorganic silica aerogel materials often have disadvantages such as poor mechanical properties and acid and alkali resistance. Melamine formaldehyde resin has excellent mechanical properties and flame retardant properties due to its high nitrogen content and high degree of cross-linking; however, due to its rigid cross-linking structure, its skeleton is brittle and difficult to resist the capillary pressure generated during the normal pressure process, making it difficult to use normal pressure drying to prepare intrinsic flame retardant melamine formaldehyde resin aerogel materials. There is currently no related work reported. Summary of the invention

[0004] In view of the above-mentioned defects, the present invention provides a method for preparing melamine formaldehyde resin by drying at normal pressure: using hydroxymethylated melamine as raw material, introducing a water-soluble polymer material as a template, firstly condensing the hydroxymethylated melamine and the polymer template in situ by a sol-gel method to grow a melamine formaldehyde resin hydrogel; and then drying the obtained hydrogel at normal pressure to obtain an aerogel. In the present invention, the addition of the polymer material can enhance the toughness of the melamine formaldehyde resin, and the melamine formaldehyde resin can greatly enhance the strength of the gel skeleton, so that it can resist the influence of surface tension on the skeleton; that is, the present invention can produce a melamine formaldehyde resin hydrogel with both toughness and strength, so that the melamine formaldehyde resin aerogel material can be prepared by the normal pressure drying method without using a solvent exchange method.

[0005] The technical solution of the present invention:

[0006] The first technical problem to be solved by the present invention is to provide a method for preparing melamine formaldehyde resin aerogel by drying at normal pressure. The preparation method comprises the following steps: firstly preparing hydrogel from hydroxymethylated melamine and a polymer template by a sol-gel method, and then preparing aerogel from the obtained hydrogel by drying at normal pressure; wherein the mass ratio of the hydroxymethylated melamine to the polymer template is 3 to 10:1, and the pH value is adjusted to be between 1 and 6 in the sol-gel method.

[0007] Furthermore, the method for preparing a hydrogel using a sol-gel method with hydroxymethylated melamine and a polymer template is as follows: firstly, hydroxymethylated melamine, a polymer template and water are mixed to prepare a mixed liquid, and the pH of the mixed liquid is adjusted to 1-6; then, the mixed liquid is reacted at 60-90° C. for 6-24 hours, and then aged at 60-90° C. for 6-24 hours.

[0008] Furthermore, the mass sum of the blended liquid prepared by hydroxymethylated melamine, polymer template and water is 100%, in which the mass ratio of hydroxymethylated melamine to polymer template is 3-10:1, and the amount of water added accounts for 70-99% of the total mass of the blended liquid.

[0009] Furthermore, in the sol-gel method, at least one of hydrochloric acid, sulfuric acid or acetic acid solution is used to adjust the pH value of the mixed liquid.

[0010] Furthermore, the normal pressure drying method is: drying the obtained hydrogel at 30-100° C. and an air circulation rate of 5 L / min-50 L / min.

[0011] Furthermore, the hydroxymethyl melamine used is synthesized from melamine and formaldehyde at a molar ratio of 1:2 to 4 under alkaline conditions (pH = 9 to 10).

[0012] Furthermore, the polymer template is a water-soluble polymer.

[0013] Furthermore, the polymer template includes: polyvinyl alcohol (which can be polypropylene alcohol nanofiber), polyacrylamide, polyvinyl pyrrolidone, polyacrylic acid, polyethylene oxide, polyvinyl alcohol, polyvinyl amine, polyacrylonitrile (which can be polypropylene nitrile nanofiber); cellulose (which can be nanocellulose fiber, carboxymethyl cellulose, aldehyde cellulose, etc.), starch (such as carboxymethyl starch, etc.), gelatin, xanthan gum, carrageenan, pectin, gellan gum, konjac gum, peach gum, tannin, cardanol, chitosan (such as carboxymethyl chitosan), carboxymethyl chitosan, lignin, glucomannan; chitin, polyester, spandex, polypropylene alcohol, silicon carbide, polyamide, alginic acid and its salts one or more. The polymer template in the present invention can use any form of the above polymer materials, such as fibers, etc.

[0014] Furthermore, in the preparation method, the raw materials also include a modifier, and the modifier includes: polyether amine (molecular weight 200-2000), polyether alcohol (molecular weight 200-2000), hydroxyl-terminated poly (dimethylsiloxane) (molecular weight 200-10000), amino-terminated poly (dimethylsiloxane) (molecular weight 200-10000); one or more of trihydroxymethylphosphine oxide, phytic acid, aminotrimethylene phosphoric acid, tannin, ammonium polyphosphate, boric acid, borax, aluminum hypophosphite, red phosphorus, and sodium phytate.

[0015] Furthermore, the amount of the modifier added is 1% to 40% of the amount of hydroxymethyl melamine added, preferably 15% to 30%.

[0016] The second technical problem to be solved by the present invention is to provide a melamine formaldehyde resin aerogel, wherein the aerogel is prepared by the above method.

[0017] Furthermore, the melamine formaldehyde resin aerogel has a density of 20 mg / cm 3 ~200mg / cm 3 .

[0018] Furthermore, the pore size distribution of the melamine formaldehyde resin aerogel is between 20 nm and 300 μm.

[0019] The third technical problem to be solved by the present invention is to point out the application of the above melamine formaldehyde resin aerogel in flame retardant materials, thermal insulation materials, fireproof materials and buffer materials.

[0020] Beneficial effects of the present invention:

[0021] The present invention provides a method for preparing melamine formaldehyde resin aerogel by drying at normal pressure. The preparation method of the present invention does not use any solvent replacement, and the aerogel material can be obtained by directly drying the hydrogel, which is simple to operate, low in cost, and has good environmental benefits and good economic benefits.

[0022] The melamine formaldehyde resin aerogel obtained by the invention has a compact structure, a shrinkage rate as low as 6%, and a density of 20 mg / cm 3 ~200mg / cm 3 , porosity is as high as 99.9%, and the pore size distribution is between 20nm and 300μm. Since the melamine formaldehyde resin aerogel obtained by the present invention has a relatively low pore size, it has excellent thermal insulation performance, and the thermal conductivity is between 12mW / (m K)-38mW / (m K). The melamine formaldehyde resin aerogel prepared by the present invention can give the melamine formaldehyde resin aerogel material excellent resilience and high modulus by adjusting the component ratio and the amount of modifier added. Among them, the compression modulus of the high-strength melamine formaldehyde resin aerogel is between 11MPa and 63MPa; the compression deformation recovery of the resilient melamine formaldehyde resin aerogel after 1000 cycles is between 90% and 100%. In addition, the melamine formaldehyde resin obtained by the present invention also has intrinsic flame retardancy, and its limiting oxygen index (LOI) is between 25% and 65%, all of which pass the vertical combustion V-0 level, and the heat release peak value is between 330 and 30 kW / m 2 The smoke release is less than 1m 2 / s, indicating that the obtained material has the potential to be used in flame retardant materials, thermal insulation materials, fireproof materials and buffer materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 are microscopic scanning electron microscope photographs of the melamine formaldehyde resin aerogel obtained in Example 3 at different magnification ratios; Figure 1 It can be seen that the aerogel prepared by normal pressure drying presents a complete three-dimensional skeleton. In the image with higher magnification, it is found that its microstructure is further aggregated by micro-nanoparticles; this special microstructure is similar to silica aerogel and is expected to give it excellent thermal insulation properties.

[0024] Figure 2 This is a digital photo of the sample obtained in Example 4. It can be seen from the picture that the aerogel prepared by normal pressure drying has good formability, exhibits low density, and can stand on the flower.

[0025] Figure 3 These are digital photos of the melamine formaldehyde resin aerogels obtained in Examples 2, 4, 10, and 11 after vertical combustion tests. The aerogels can pass the vertical combustion V-0 grade and exhibit excellent charring performance.

[0026] Figure 4 A digital photo of the sample is obtained for Comparative Example 1; Figure 4It can be seen that: in the absence of a polymer template, the same preparation method cannot successfully prepare melamine formaldehyde resin aerogel, and the material shows large skeleton collapse and cracking. The polymer template in the present invention plays a vital role in enhancing the gel skeleton, strength and toughness, and can help resist the negative effects of capillary tension during the gel drying process and avoid gel structure collapse and shrinkage.

[0027] Figure 5 A digital photo of the sample is obtained for Comparative Example 2; Figure 5 It can be seen that pure polymer templates cannot be directly dried at normal pressure to prepare aerogel materials, because the polymer templates are too tough and have low skeleton strength, so during the drying process, their skeletons are difficult to resist capillary tension; and melamine formaldehyde resin has a large number of rigid triazine rings, which can greatly enhance the strength of the material to resist capillary tension; therefore, in the present invention, both the polymer template and the melamine formaldehyde resin are the key to the successful preparation of aerogels.

[0028] Figure 6 A digital photo of the sample is obtained for Comparative Example 3; Figure 6 It can be seen that when the polymer template and melamine formaldehyde resin are used to prepare aerogel in a mass ratio greater than 1:2, a structurally complete aerogel material cannot be obtained. This is because the melamine formaldehyde resin is relatively small under this condition, and the gel skeleton strength is still difficult to resist the capillary tension, and the material breaks. Only when the mass ratio of the two is less than 1:3, a complete aerogel material can be obtained, and as the ratio of melamine formaldehyde resin increases, the integrity of the aerogel becomes better and the overall performance is also better. This shows that only when the amount of melamine formaldehyde resin added is high, the skeleton strength is more suitable for the preparation of aerogel material by normal pressure drying.

[0029] Figure 7 Digital photos of samples obtained for Comparative Examples 4 (pH=7), 5 (pH=0.1), 6 (pH not adjusted) and Example 2 (pH=3); Figure 7 It can be seen that in the sol-gel process, the pH value of the system is a crucial condition for the preparation of complete aerogels. Only under acidic conditions can the hydrogel structure prepared by sol-gel be denser and more uniform. At this time, it can better resist capillary tension and thus achieve the preparation of structurally complete aerogels. DETAILED DESCRIPTION

[0030] The present invention uses a polymer material as a template and adopts a sol-gel method to in-situ condense and grow hydroxymethylated melamine to obtain a melamine formaldehyde resin aerogel skeleton. The addition of the polymer material can enhance the toughness of the melamine formaldehyde resin, and the melamine formaldehyde resin can greatly enhance the strength of the gel skeleton, so that it can resist the influence of surface tension on the skeleton. The preparation method of the present invention obtains a melamine formaldehyde resin with both toughness and strength by regulating the skeleton strength and pore size distribution, so that the melamine formaldehyde resin aerogel material can be prepared by drying at normal pressure without using solvent exchange. In addition, the preparation method of the present invention is simple to operate, low in cost, has good environmental benefits, and has good economic benefits.

[0031] The melamine formaldehyde resin aerogel obtained by the present invention has a relatively low pore size (10nm-300μm), so that it has excellent thermal insulation performance, and the thermal conductivity coefficient is between 12mW / (m K)-38mW / (m K). In addition, the melamine formaldehyde resin obtained by the present invention also has intrinsic flame retardancy, and its limiting oxygen index is between 25% and 65%, and it passes the vertical combustion V-0 level, and the heat release peak is between 330kW / m 2 The smoke release is less than 1m 2 / s. This indicates that the obtained material has the potential to be used in flame retardant materials and thermal insulation materials.

[0032] The specific implementation modes of the present invention are further described below in conjunction with embodiments, but the present invention is not limited to the scope of the embodiments.

[0033] Materials and reagents used in the embodiments of the present invention: Nanocellulose fibers were purchased from Zhejiang Jinjiahao Green Nanomaterials Co., Ltd. (solid content was 1 wt%); melamine, formaldehyde, sulfuric acid, and acetic acid were purchased from Sichuan Cologne Reagent Co., Ltd.; polyvinyl alcohol, gelatin, sodium alginate, and carboxymethyl chitosan were all purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0034] In the present invention, the limiting oxygen index is tested by GB / T 2046.2-2009, and the vertical combustion is tested by GB / T2408-2008; the mechanical property test is carried out by using an American Instron 3366 electronic universal material testing machine to test the mechanical properties of the material; the thermal conductivity is tested by using a TPS2500 (Hot Disk, Sweden) thermal conductivity meter; the peak heat release is tested by using a Fire Testing Technology standard cone calorimeter (FTT StandardCone Calorimeter) according to standard ISO5660-1, and the radiation power is 50kW / m 2The microstructure of the aerogel was characterized by a JEOL JSM-5900LV scanning electron microscope. The pore size distribution was tested by mercury intrusion porosimetry (MIP). The porosity and pore size distribution of the aerogel were tested by Auto Pore IV 9500 mercury intrusion instrument, and the micropore size distribution and specific surface area of ​​the aerogel were determined by a Quantachrome 2000e fully automatic specific surface and porosity analyzer.

[0035] Example 1

[0036] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 7.5:2.5:90, and the pH value of the solution was adjusted to 5 using sulfuric acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 10 L / min to obtain the final product.

[0037] The density of this product is 103mg / cm 3 , limiting oxygen index is 36%, vertical combustion V-0, peak heat release is 112kW / m 2 , compression modulus is 18MPa, thermal conductivity is 28mW / (m K), and pore size is 30nm-80nm.

[0038] Example 2

[0039] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 3.2:0.8:96, and the pH value of the solution was adjusted to 6 with sulfuric acid. The mixture was reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours to obtain a hydrogel. The hydrogel was taken out and dried at 80°C with an air flow rate of 15L / min to obtain the final product, melamine formaldehyde resin aerogel.

[0040] The density of the obtained aerogel is 53 mg / cm 3 , limiting oxygen index is 35%, vertical combustion V-0, peak heat release is 110kW / m 2 The compression modulus is 0.2MPa, the thermal conductivity is 21mW / (m K), and the pore size is 18nm-64nm. The aerogel has resilience. After being compressed 10 times at 50% deformation, the deformation retention rate is 98% and the strength retention rate is 50%.

[0041] Example 3

[0042] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 4:1:95, and the pH value of the solution was adjusted to 3 using sulfuric acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 10 L / min to obtain the final product.

[0043] The density of this product is 59mg / cm 3 , limiting oxygen index is 35%, vertical combustion V-0, peak heat release is 105kW / m 2 The compression modulus is 0.8MPa, the thermal conductivity is 21mW / (m K), and the pore size is 90nm-120nm. The aerogel has resilience. After being compressed 10 times at 50% deformation, the deformation retention rate is 98% and the strength retention rate is 92%.

[0044] Example 4

[0045] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 9.6:2.4:88, the pH value of the solution was adjusted to 5 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 70°C with an air flow rate of 10L / min to obtain the final product.

[0046] The density of this product is 112mg / cm 3 , limiting oxygen index is 36%, vertical combustion V-0, peak heat release is 120kW / m 2 Aerogel has hard characteristics, compression modulus of 29MPa, thermal conductivity of 28mW / (m K), pore size of 80nm-110nm, appearance morphology Figure 2 shown.

[0047] Example 5

[0048] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 20:5:75, and the pH value of the solution was adjusted to 5 using sulfuric acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 20 L / min to obtain the final product.

[0049] The density of this product is 198mg / cm 3 , limiting oxygen index is 37%, vertical combustion V-0, peak heat release is 160kW / m 2 , compression modulus is 60MPa, thermal conductivity is 38mW / (m K), and pore size is 120nm-600nm.

[0050] Example 6

[0051] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 6.6:1.4:92, and the pH value of the solution was adjusted to 4 using sulfuric acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 40 L / min to obtain the final product.

[0052] The density of this product is 82mg / cm 3 , limiting oxygen index is 36%, vertical combustion V-0, peak heat release is 101kW / m 2 , compression modulus is 24MPa, thermal conductivity is 22mW / (m K), and pore size is 40nm-100nm.

[0053] Example 7

[0054] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 4.3:0.7:95, and the pH value of the solution was adjusted to 5 using sulfuric acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 75°C with an air flow rate of 10 L / min to obtain the final product.

[0055] The density of this product is 46mg / cm 3 , limiting oxygen index is 35%, vertical combustion V-0, peak heat release is 95kW / m 2 , compression modulus is 0.8MPa, thermal conductivity is 18mW / (m K), and pore size is 18nm-70nm.

[0056] Example 8

[0057] Hydroxymethylated melamine, polyvinyl alcohol and water were mixed in a mass ratio of 5:1:94, and the pH value of the solution was adjusted to 5 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 100°C with an air flow rate of 10L / min to obtain the final product.

[0058] The product has a limiting oxygen index of 32%, vertical combustion V-0, and a peak heat release of 330kW / m 2 , compression modulus is 34MPa, thermal conductivity is 23mW / (m K), pore size is 80nm-100nm

[0059] Example 9

[0060] Hydroxymethylated melamine, polyvinyl alcohol and water were mixed in a mass ratio of 12:3:85, and the pH value of the solution was adjusted to 5 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 100°C with an air flow rate of 10L / min to obtain the final product.

[0061] The product has a limiting oxygen index of 36%, vertical combustion V-0, and a peak heat release of 210kW / m 2 , compression modulus is 24MPa, thermal conductivity is 22mW / (m K), pore size is 40nm-100nm

[0062] Example 10

[0063] Hydroxymethylated melamine, polyvinyl alcohol, amino-terminated polysiloxane (molecular weight 500) and water were mixed in a mass ratio of 6:1:2:91, and the pH value of the solution was adjusted to 3 with acetic acid, and then reacted in a sealed container at 95°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 5L / min to obtain the final product.

[0064] The product has a limiting oxygen index of 35.5%, vertical combustion V-0, and a peak heat release of 280kW / m 2 , compression modulus is 26.5MPa, thermal conductivity is 18mW / (m K), and pore size is 10nm-80nm.

[0065] Embodiment 11

[0066] Hydroxymethylated melamine, gelatin, trishydroxymethylphosphine oxide and water were mixed in a mass ratio of 7:2:1:90, the pH value of the solution was adjusted to 2 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 60°C with an air flow rate of 15L / min to obtain the final product.

[0067] The product has a limiting oxygen index of 40.5%, vertical combustion V-0, and a peak heat release of 60kW / m 2 , compression modulus is 33MPa, thermal conductivity is 26mW / (m K) and pore size is 60nm-110nm.

[0068] Example 12

[0069] Hydroxymethylated melamine, gelatin, red phosphorus and water were mixed in a mass ratio of 8:1.5:0.5:90, and the pH value of the solution was adjusted to 3 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 60°C with an air flow rate of 15L / min to obtain the final product.

[0070] The product has a limiting oxygen index of 42.5%, vertical combustion V-0, and a peak heat release of 30kW / m 2 , compression modulus is 28MPa, thermal conductivity is 31mW / (m K), and pore size is 100nm-310nm.

[0071] Embodiment 13

[0072] Hydroxymethylated melamine, chitin nanofibers and water were mixed in a mass ratio of 8:2:90, and the pH value of the solution was adjusted to 4 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 60°C with an air flow rate of 15L / min to obtain the final product.

[0073] The product has a limiting oxygen index of 34.5%, vertical combustion V-0, and a peak heat release of 160kW / m 2 , compression modulus is 43MPa, thermal conductivity is 28mW / (m K), and pore size is 50nm-110nm.

[0074] Embodiment 14

[0075] Hydroxymethylated melamine, polyacryl alcohol nanofibers and water were mixed in a mass ratio of 9:1:90, and the pH value of the solution was adjusted to 3 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 60°C with an air flow rate of 15L / min to obtain the final product.

[0076] The product has a limiting oxygen index of 32.5%, vertical combustion V-0, and a peak heat release of 300kW / m 2 , compression modulus is 34MPa, thermal conductivity is 27mW / (m K), and pore size is 40nm-80nm.

[0077] Embodiment 15

[0078] Hydroxymethylated melamine, sodium alginate, sodium phytate and water were mixed in a mass ratio of 8:1:1:90, and the pH value of the solution was adjusted to 3 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 60°C with an air flow rate of 15L / min to obtain the final product.

[0079] The product has a limiting oxygen index of 39.5%, vertical combustion V-0, and a peak heat release of 80kW / m 2 , compression modulus is 63MPa, thermal conductivity is 24mW / (m K), pore size is 50nm-95nm

[0080] Example 16

[0081] Hydroxymethylated melamine, carboxymethyl chitosan and water were mixed in a mass ratio of 4:1:95, and the pH value of the solution was adjusted to 3 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 60°C with an air flow rate of 50L / min to obtain the final product.

[0082] The product has a limiting oxygen index of 38%, vertical combustion V-0, and a peak heat release of 110kW / m 2 , compression modulus is 35MPa, thermal conductivity is 19mW / (m K), and pore size is 20nm-60nm.

[0083] Embodiment 17

[0084] Hydroxymethylated melamine, carboxymethyl chitosan and water were mixed in a mass ratio of 6:2:92, and the pH value of the solution was adjusted to 4 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 10L / min to obtain the final product.

[0085] The product has a limiting oxygen index of 39%, vertical combustion V-0, and a peak heat release of 108kW / m 2 , compression modulus is 41MPa, thermal conductivity is 22mW / (m K), and pore size is 60nm-80nm.

[0086] Embodiment 18

[0087] Hydroxymethylated melamine, carboxymethyl chitosan and water were mixed in a mass ratio of 14:2:84, and the pH value of the solution was adjusted to 5 with acetic acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 70°C with an air flow rate of 15L / min to obtain the final product.

[0088] The product has a limiting oxygen index of 41%, vertical combustion V-0, and a peak heat release of 160kW / m 2 , compression modulus is 63MPa, thermal conductivity is 31mW / (m K), and pore size is 120nm-550nm.

[0089] Comparative Example 1:

[0090] Mix hydroxymethylated melamine and water in a mass ratio of 10:90, adjust the pH value of the solution to 5 with sulfuric acid, and then react in a sealed container at 90°C for 24 hours, and then continue to age at room temperature for 24 hours. Take out the gel and dry it at 80°C with an air flow rate of 10L / min to obtain the final product. Its appearance result is as follows Figure 4 shown.

[0091] Comparative Example 2:

[0092] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 2.5:7.5:90, and the pH value of the solution was adjusted to 5 with sulfuric acid. The mixture was then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 10 L / min to obtain the final product. The appearance result is as follows: Figure 5 shown.

[0093] Comparative Example 3:

[0094] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 5:5:90, and the pH value of the solution was adjusted to 5 using sulfuric acid. The mixture was then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 10 L / min to obtain the final product. The appearance result is as follows: Figure 6 shown.

[0095] Comparative Example 4:

[0096] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 7.5:2.5:90, and the pH value of the solution was adjusted to 7 with sulfuric acid. The mixture was then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 10 L / min to obtain the final product. The appearance result is as follows: Figure 7 shown.

[0097] Comparative Example 5:

[0098] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 7.5:2.5:90, and the pH value of the solution was adjusted to 0.1 with sulfuric acid. The mixture was then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 10 L / min to obtain the final product. The appearance result is as follows: Figure 7 shown.

[0099] Comparative Example 6:

[0100] The hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 7.5:2.5:90, and then directionally frozen in a liquid nitrogen bath, and then freeze-dried in a freeze dryer. The dried sample was placed in a vacuum oven at 80°C for 24 hours to obtain the final product.

[0101] The product has a limiting oxygen index of 35.5%, vertical combustion V-0, a compression modulus of 46MPa, and a peak heat release of 110kW / m 2 , thermal conductivity is 45mW / (m K) and pore size is 200μm.

[0102] Comparative Example 7:

[0103] Hydroxymethylated melamine, nanocellulose fibers and water were mixed in a mass ratio of 7.5:2.5:90, and the pH value of the solution was adjusted to 5 with sulfuric acid, and then reacted in a sealed container at 90°C for 24 hours, and then aged at room temperature for 24 hours, and solvent replaced with ethanol (the mass ratio of sample to ethanol was 1:10) for 24 hours. The gel was taken out and dried at 80°C with an air flow rate of 10L / min to obtain the final product.

[0104] The product has a limiting oxygen index of 35.5%, a vertical combustion V-0, a compression modulus of 15MPa, and a peak heat release of 110kW / m 2 , thermal conductivity is 30mW / (m K), and pore size is 50-100μm.

[0105] Table 1 Preparation conditions of each embodiment and comparative example

[0106]

[0107]

[0108] Note: A in the table = melamine formaldehyde resin; except for comparative example 6, which was dried by freeze drying, the drying methods used in the other embodiments and comparative examples were all dried at normal pressure; except for comparative example 7, which was subjected to solvent replacement, the other embodiments and comparative examples were not subjected to solvent replacement.

[0109] Table 2 Performance test results of samples obtained from various embodiments and comparative examples

[0110]

Claims

1. A method for preparing melamine formaldehyde resin aerogel by drying at normal pressure, characterized in that: The method comprises: firstly mixing hydroxymethylated melamine, a polymer template and water to obtain a mixed liquid, and adjusting the pH value of the mixed liquid to be between 1 and 6; then reacting at 60 to 90° C. for 6 to 24 hours, and then aging at 60 to 90° C. for 6 to 24 hours to obtain a hydrogel, and then drying the obtained hydrogel at normal pressure to obtain an aerogel; wherein the polymer template is a water-soluble polymer, and the mass ratio of hydroxymethylated melamine to the polymer template is 3 to 10:1; and the normal pressure drying method comprises: drying the obtained hydrogel at 30 to 100° C. and an air circulation speed of 5 L / min to 50 L / min.

2. The method for preparing melamine formaldehyde resin aerogel by drying at normal pressure according to claim 1, characterized in that: The total mass of the mixed liquid prepared from the hydroxymethylated melamine, the polymer template and water is 100%, and the amount of water added accounts for 70-99% of the total mass of the mixed liquid.

3. The method for preparing melamine formaldehyde resin aerogel by drying at normal pressure according to any one of claims 1 to 2, characterized in that: The pH of the blend is adjusted using hydrochloric acid, sulfuric acid or acetic acid.

4. The method for preparing melamine formaldehyde resin aerogel by drying at normal pressure according to any one of claims 1 to 2, characterized in that: The hydroxymethyl melamine used is synthesized from melamine and formaldehyde in an amount ratio of 1:2 to 4 under alkaline conditions.

5. The method for preparing melamine formaldehyde resin aerogel by drying at normal pressure according to any one of claims 1 to 2, characterized in that: The polymer template includes: polyvinyl alcohol, polyacrylamide, polyvinyl pyrrolidone, polyacrylic acid, polyethylene oxide, polyvinyl alcohol, polyvinyl amine, polyacrylonitrile; cellulose, starch, gelatin, xanthan gum, carrageenan, pectin, gellan gum, konjac gum, peach gum, tannin, cardanol, chitosan, carboxymethyl chitosan, lignin, glucomannan; chitosan, polyester, spandex, polypropylene alcohol, polyamide, alginic acid and its salts or one or more.

6. The method for preparing melamine formaldehyde resin aerogel by drying at normal pressure according to any one of claims 1 to 2, characterized in that: In the preparation method, the raw materials also include a modifier, and the modifier includes: polyetheramine, polyether alcohol, hydroxyl-terminated poly(dimethylsiloxane), amino-terminated poly(dimethylsiloxane); one or more of trihydroxymethylphosphine oxide, phytic acid, aminotrimethylene phosphoric acid, tannin, ammonium polyphosphate, boric acid, borax, aluminum hypophosphite, red phosphorus or sodium phytate.

7. The method for preparing melamine formaldehyde resin aerogel by drying at normal pressure according to claim 6, characterized in that: The amount of the modifier added is 1% to 40% of the mass of the hydroxymethyl melamine.

8. The method for preparing melamine formaldehyde resin aerogel by drying at normal pressure according to claim 7, characterized in that: The addition amount of the modifier is 15% to 30%.

9. A melamine formaldehyde resin aerogel, characterized in that: The melamine formaldehyde resin aerogel is prepared by the method according to any one of claims 1 to 8.

10. Application of melamine formaldehyde resin aerogel in flame retardant materials, thermal insulation materials, fireproof materials and buffer materials, characterized in that: The melamine formaldehyde resin aerogel is a melamine formaldehyde resin aerogel prepared by the method according to any one of claims 1 to 8, or is the melamine formaldehyde resin aerogel according to claim 9.