A polycrystalline SiC molded body, a manufacturing method thereof and a plasma etching method
By controlling the main surface corrugation and grinding method of the polycrystalline SiC molded body, the problem of unevenness of the etching of semiconductor wafers is solved, and a uniform etching effect is achieved, and suitable for other applications with high flatness requirements.
Patent Information
- Application Number
- CN202280008272.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-10-28
- Filing Date
- 2022-09-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-09-26
AI Technical Summary
When manufacturing semiconductor devices, the increase in the area of the semiconductor wafer and the increase in circuit density lead to uneven plasma etching, and the smoothness of the electrode surface has a great impact on the etching uniformity, making it difficult for the prior art to achieve uniform plasma etching.
The smoothness and uniformity of the electrode are ensured by extracting the arithmetic average wrigility of a specific wavelength range from the main surface cross-section curve of the polycrystalline SiC molded body, and controlling the wrigility within a specific range through a multi-stage grinding method.
A polycrystalline SiC molded body with good uniformity in plasma etching and its manufacturing method are realized, which reduces etch marks and is suitable for other uses with high flatness requirements, such as the support of a single crystal SiC substrate.
Smart Images

Figure GDA0004289800930000091 
Figure GDA0004289800930000101 
Figure GDA0004289800930000102
Abstract
Description
Technical Field
[0001] The present invention relates to a polycrystalline SiC molded body and a method for producing the same. Background Art
[0002] Polycrystalline SiC molded bodies are excellent in various properties such as heat resistance, corrosion resistance and strength, and are used for various purposes. For example, Patent Document 1 (Japanese Patent Publication No. 2001-220237) describes the use of silicon carbide (SiC) as an electrode of a plasma etching device used in the manufacture of semiconductor devices.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2001-220237. Summary of the invention
[0006] Problems to be solved by the invention
[0007] As the area of semiconductor wafers used in manufacturing semiconductor devices increases, the density of circuits formed therein increases. Therefore, a technique for more uniformly etching semiconductor wafers is required for plasma etching performed when manufacturing semiconductor devices.
[0008] Regarding electrodes used in plasma etching, in addition to the uniformity of resistivity (Patent Document 1) and uniformity of thermal conductivity, the smoothness of the electrode surface also affects the uniformity of plasma etching. Therefore, the object of the present invention is to provide a polycrystalline SiC molded body and a method for manufacturing the same that can achieve uniform plasma etching when used as an electrode.
[0009] Means of solving problems
[0010] The present inventors have found that the above-mentioned problems can be solved by extracting a waviness curve from a cross-sectional curve of a main surface of a polycrystalline SiC molded body, obtaining an arithmetic mean waviness from a specific wavelength component in the waviness curve, and limiting the arithmetic mean waviness to a specific range. That is, the present invention provides the following.
[0011] One embodiment of the present invention is a polycrystalline SiC molded body having two relative main surfaces, wherein, with respect to an arithmetic mean waviness Wa corresponding to a specified wavelength range and extracted from a cross-sectional curve of the main surfaces, when the wavelength range is 0 to 10 mm, the Wa is less than 0.05 μm; when the wavelength range is 10 to 20 mm, the Wa is less than 0.13 μm; when the wavelength range is 20 to 30 mm, the Wa is less than 0.20 μm.
[0012] In addition, one embodiment of the present invention is a method for manufacturing the above-mentioned polycrystalline SiC molded body, the method comprising: a step of forming a polycrystalline SiC film having a main surface; a step of grinding the main surface of the polycrystalline SiC film. The grinding step comprises: a step of grinding the main surface by a first grinding material; a step of grinding the main surface by a second grinding material after the step of grinding by the first grinding material; a step of grinding the main surface by a third grinding material after the step of grinding by the second grinding material. The particle size of the first grinding material is coarser than that of the second grinding material, and the particle size of the second grinding material is coarser than that of the third grinding material.
[0013] Effects of the Invention
[0014] According to the present invention, a polycrystalline SiC molded body capable of achieving uniform plasma etching when used as an electrode and a method for producing the same can be provided. DETAILED DESCRIPTION
[0015] Embodiments of the present invention will be described below.
[0016] (Polycrystalline SiC molded body)
[0017] The polycrystalline SiC molded body of the present embodiment has two main faces relative to each other. The two main faces include a first main face and a second main face. In the present application specification, the main face refers to a substantially flat surface. Regarding the arithmetic mean waviness Wa corresponding to the specified wavelength range extracted from the cross-sectional curve of the main face, when the wavelength range is 0 to 10 mm, Wa is less than 0.05 μm; when the wavelength range is 10 to 20 mm, Wa is less than 0.13 μm; when the wavelength range is 20 to 30 mm, Wa is less than 0.20 μm.
[0018] Here, the definitions of "cross-sectional curve" and "arithmetic mean waviness" are based on JIS B 0601. For example, when extracting the wavelength range of 0 to 10 mm from the cross-sectional curve, the cross-sectional curve frequency is expanded and 1×10 3 The frequency at which the vibration transmissibility of the frequency component above 10000 m is 50% is set as a critical value, and the arithmetic mean waviness is derived. In this case, the frequency extension is preferably performed by Fourier transform.
[0019] The arithmetic mean waviness Wa (hereinafter referred to as “Wa (0-10 mm)”) in the wavelength range of 0-10 mm is calculated based on the spatial frequency of the cross-sectional curve being 1 (×10 3 / m) and above.
[0020] The arithmetic mean waviness Wa (hereinafter referred to as "Wa (10-20 mm)") in the wavelength range of 10-20 mm is calculated based on the spatial frequency of the cross-sectional curve of 1 / 2 to 1 (×10 3 / m) components to obtain the arithmetic mean waviness.
[0021] The arithmetic mean waviness Wa (hereinafter referred to as “Wa (20-30 mm)”) in the wavelength range of 20-30 mm is calculated based on the spatial frequency of the cross-sectional curve of 1 / 3 to 1 / 2 (×10 3 / m) components to obtain the arithmetic mean waviness.
[0022] According to the present embodiment, as described above, by using a polycrystalline SiC molded body having specific Wa (0 to 10 mm), specific Wa (10 to 20 mm), and specific Wa (20 to 30 mm) as an electrode, it is possible to achieve uniform plasma etching with few traces.
[0023] In addition, the polycrystalline SiC molded body of the present embodiment has a main surface with high flatness. Therefore, the polycrystalline SiC molded body of the present embodiment can be used not only as an electrode of a plasma etching device, but also suitable for other uses requiring flatness. For example, the polycrystalline SiC molded body of the present embodiment is sometimes bonded to a single crystal SiC substrate and used as a supporting substrate for the single crystal SiC substrate. In such uses, the polycrystalline SiC molded body is required to have a flat surface. The polycrystalline SiC molded body of the present embodiment has a flat main surface. Therefore, it can also be suitable for uses in bonding with a single crystal SiC substrate.
[0024] Preferably, the polycrystalline SiC molded body is in the shape of a disk. That is, the main surface of the polycrystalline SiC molded body is circular. More preferably, the polycrystalline SiC molded body is in the shape of a disk, and the main surface diameter of the polycrystalline SiC molded body is 1.5 to 20 inches, and more preferably 6 to 18 inches.
[0025] Preferably, the thickness of the polycrystalline SiC molded body is 0.1 to 4.0 mm.
[0026] (Method for producing polycrystalline SiC molded body)
[0027] Next, a method for producing a polycrystalline SiC molded body according to the present embodiment will be described.
[0028] The manufacturing method of this embodiment includes: forming a polycrystalline SiC film having a main surface (step S1), and polishing the main surface of the polycrystalline SiC film (step S2). Each step will be described in detail below.
[0029] Step S1: Formation of polycrystalline SiC film
[0030] The polycrystalline SiC film can be formed by, for example, a CVD method. The film formation conditions are not particularly limited, and known conditions (for example, Japanese Patent Application Laid-Open No. 2021-54666) can be adopted.
[0031] For example, first, a graphite substrate or the like is placed in a CVD furnace as a base material.
[0032] After that, the carrier gas and the raw material gas as the SiC supply source are mixed, and a nitrogen-containing gas is added as needed, and the mixed gas is supplied to the CVD furnace. The substrate surface temperature is set to generate polycrystalline SiC from the raw material gas. Thus, a polycrystalline SiC layer is formed on the substrate. In addition, when a nitrogen-containing gas is used, nitrogen can be doped into the polycrystalline SiC layer.
[0033] After the polycrystalline SiC layer is formed, the obtained polycrystalline SiC layer is separated from the substrate, thereby obtaining a polycrystalline SiC film having two main surfaces (ie, a first main surface and a second main surface).
[0034] The polycrystalline SiC film obtained as described above preferably has a volume resistivity of 0.050Ωcm or less. With such a volume resistivity, when used as an electrode for plasma etching, the volume resistivity of the polycrystalline SiC film can effectively release static electricity and uniformly generate plasma gas. In addition, when used as an electrode for plasma etching, from the perspective of ensuring a high etching rate, the volume resistivity of the polycrystalline SiC film is preferably 0.030Ωcm or less, and more preferably 0.020Ωcm or less.
[0035] The volume resistivity can be adjusted by, for example, allowing the polycrystalline SiC film to contain a predetermined amount of nitrogen. By increasing the nitrogen content, the volume resistivity can be reduced.
[0036] The nitrogen content of the polycrystalline SiC film is, for example, 200 ppm (mass parts per million) or more, preferably 200 to 1000 ppm (mass parts per million). When the nitrogen content is in this range, the degree of change in resistivity relative to the change in nitrogen content becomes smaller. Therefore, by controlling the nitrogen content of the polycrystalline SiC film, the desired volume resistivity can be easily obtained. In addition, if the nitrogen content is less than 1000 ppm (mass parts per million), the crystal defects caused by the introduction of nitrogen will hardly affect the flatness of the polycrystalline SiC film.
[0037] In addition, the method of introducing nitrogen is not particularly limited. For example, as described above, when a polycrystalline SiC film is formed by a CVD method, nitrogen can be introduced into the formed polycrystalline SiC film using a nitrogen-containing gas.
[0038] Step S2: Grinding
[0039] Next, the two main surfaces of the obtained polycrystalline SiC film are polished. Here, the main surfaces are polished in three stages (steps S2-1 to S2-3) described below.
[0040] [Step S2-1]
[0041] First, the main surface of the polycrystalline SiC film is ground by a first grinding material. Specifically, the polycrystalline SiC film is placed on a supporting substrate (such as a metal plate) and fixed to the supporting substrate with a first fixing material. At this time, the polycrystalline SiC film is fixed to the supporting substrate in a form where one main surface side is not fixed. After that, the main surface of the unfixed polycrystalline SiC film is ground by the first grinding material. After grinding one main surface, remove the polycrystalline SiC substrate from the supporting substrate. After that, the other main surface is ground in the same way. The second main surface can be ground after the first main surface is ground. The first main surface can also be ground after the second main surface is ground.
[0042] Here, the polycrystalline SiC film can be fixed on the support substrate, for example, in the following order. First, the support substrate and the polycrystalline SiC film are heated to about 100°C on a heating plate, and then a fixing material (such as a thermoplastic resin) is arranged between the support substrate and the polycrystalline SiC film, and the fixing material is softened by heat conducted from the heating plate, so that the polycrystalline SiC film is bonded to the support substrate. Next, the heating of the heating plate is stopped, and the support substrate and the polycrystalline SiC film fixed thereon are cooled to solidify the fixing material, thereby fixing the polycrystalline SiC film on the support substrate.
[0043] As the first abrasive material, for example, a cup wheel or abrasive powder can be used.
[0044] In addition, as the first abrasive, for example, when using abrasive powder, an abrasive having a relatively coarse particle size (for example, #50 to #500) is used. Here, the definition of "particle size" is based on JIS R 6001-1 and JIS R 6001-2.
[0045] As the first fixing material, for example, a thermoplastic resin is used.
[0046] In addition, as the first fixing material, it is preferable to use a material having a Mooney viscosity of 30 to 60M.
[0047] Here, Mooney viscosity is expressed in Mooney units (M). Mooney units refer to the units indicated or recorded by a torque indicating device used in a viscosity test and a Mooney scorch test based on JIS K 6300-1. Specifically, when the torque acting on the rotor shaft is 8.30 N·m, it is referred to as 100 Mooney units (100 M).
[0048] [Step S2-2]
[0049] Next, the polycrystalline SiC film is removed from the support substrate, and the first fixing material on the support substrate is removed. After that, the polycrystalline SiC film is fixed to the support substrate by the second fixing material in the same manner as step S2-1. Then, the main surface of the polycrystalline SiC film is polished by the second polishing material.
[0050] As the second abrasive, a cup wheel or abrasive powder can be used similarly to the first abrasive.
[0051] Here, the particle size of the second abrasive is finer than that of the first abrasive. For example, in the case of abrasive powder, the particle size of the second abrasive is greater than #500 and less than or equal to #5000.
[0052] As the second fixing material, a thermoplastic resin or the like can be used similarly to the first fixing material.
[0053] Here, as the second fixing material, it is preferable to use a material having a Mooney viscosity greater than that of the first fixing material. The Mooney viscosity of the second fixing material is, for example, 60 to 80M.
[0054] [Step S2-3]
[0055] Finally, similarly to step S2-2, the polycrystalline SiC film is removed from the support substrate, and the second fixing material on the support substrate is removed. Thereafter, the polycrystalline SiC film is fixed to the support substrate by the third fixing material in the same manner as step S2-1. Then, the main surface of the polycrystalline SiC film is polished by the third polishing material.
[0056] As the third abrasive, a cup wheel or abrasive powder can be used similarly to the first abrasive and the second abrasive.
[0057] Here, the particle size of the third abrasive is finer than that of the second abrasive. For example, in the case of abrasive powder, the particle size of the third abrasive is greater than #5000 and less than or equal to #50000.
[0058] As the third fixing material, a thermoplastic resin or the like can be used similarly to the first fixing material and the second fixing material.
[0059] Here, the Mooney viscosity of the third fixing material is preferably greater than that of the second fixing material. The Mooney viscosity of the third fixing material is, for example, 80 to 120M.
[0060] As described above, the present embodiment changes the grinding material and the fixing material, and implements the grinding steps of step S2-1 to step S2-3. As a result, the unevenness (low spatial frequency) between positions separated to a certain extent on the main surface of the polycrystalline SiC film and the morphological unevenness (high spatial frequency) between the adjacent precipitated grains are flattened. As a result, a polycrystalline SiC molded body with a specific Wa (0 to 10 mm), a specific Wa (10 to 20 mm), and a specific Wa (20 to 30 mm) can be obtained.
[0061] Example
[0062] In order to explain the present invention in more detail, the following examples implemented by the inventors are described. However, the present invention should not be limited to the following examples for interpretation.
[0063] (Fabrication of Polycrystalline SiC Film)
[0064] A disk-shaped graphite substrate with a diameter of 220 mm and a thickness of 5 mm was placed in the CVD furnace. Trimethylchlorosilane as a raw material gas, hydrogen as a carrier gas, and nitrogen were introduced into the CVD furnace, and the substrate temperature was set to 1500°C for 10 hours to form a polycrystalline SiC film on the graphite substrate.
[0065] In addition, the concentration of the raw material gas is changed between the initial film formation period (from the start of film formation to 2.5 hours), the middle film formation period (from 2.5 hours to 5 hours after the start of film formation), and the late film formation period (from 5 hours to 10 hours after the start of film formation). Specifically, the raw material gas concentration (first concentration) in the initial film formation period is set to 9.0 vol%, and the raw material gas concentration (second concentration) in the late film formation period is set to 7.5 vol%.
[0066] That is, the ratio of the raw material gas concentration at the initial stage of film formation to the raw material gas concentration at the later stage of film formation (referred to as the raw material gas concentration ratio) is set to 1.2 times. In addition, in the middle stage of film formation, the raw material gas concentration is reduced at a fixed rate from the concentration at the initial stage of film formation to the concentration at the later stage of film formation. In addition, the raw material gas flow rate and the carrier gas flow rate are controlled so that the total value of the raw material gas flow rate and the carrier gas flow rate is constant (140 L / min.).
[0067] The nitrogen gas flow rate was set constant throughout the film formation period. Specifically, the nitrogen gas flow rate was set to 17.5 (L / min.).
[0068] The gas residence time is 44.1 (seconds). In addition, the gas residence time is calculated by the following formula.
[0069] (Formula 1): Gas residence time (seconds) = (furnace volume / gas flow rate) × [(20 + 273) / (reaction temperature + 273)] × 60
[0070] After the polycrystalline SiC film was formed, the graphite substrate was taken out of the CVD furnace and subjected to peripheral processing and cutting processing. Then, the graphite substrate was removed to obtain a disk-shaped polycrystalline SiC film with a diameter of 205 mm and a thickness of 0.6 mm.
[0071] The two main surfaces of the obtained polycrystalline SiC film were polished under the conditions shown in Examples 1 to 3 and Comparative Examples 1 to 5 below (Table 1) to prepare electrodes for plasma etching.
[0072] Here, a thermoplastic resin with a Mooney viscosity of 45M was used as the first fixing material, and a grinding powder with an average particle size of #200 was used as the first grinding material. In addition, a thermoplastic resin with a Mooney viscosity of 70M was used as the second fixing material, and a grinding powder with an average particle size of #3000 was used as the second grinding material. Furthermore, a thermoplastic resin with a Mooney viscosity of 100M was used as the third fixing material, and a grinding powder with an average particle size of #40000 was used as the third grinding material.
[0073] As a support substrate for fixing the polycrystalline SiC film during polishing, a flat iron-based metal plate with high thermal conductivity was used.
[0074] On the other hand, when the first fixing material, the second fixing material or the third fixing material is not used as the fixing material, a porous clamp is used to fix the fixing material on the adsorption workbench by adsorption.
[0075] (Measurement method of Wa)
[0076] The cross-sectional curve of the main surface of the polycrystalline SiC film, the extraction of three wavelength ranges (0-10 mm, 10-20 mm, 20-30 mm) from the cross-sectional curve, and the arithmetic mean waviness corresponding to each extracted wavelength [Wa (0-10 mm), Wa (10-20 mm), Wa (20-30 mm)] were measured and calculated using FlatMaster produced by Corning Tropel.
[0077] (Evaluation method of etching non-uniformity)
[0078] The polycrystalline SiC film processed into a plasma etching electrode is set as an electrode in the etching device, and a voltage is applied to generate CF4 plasma. A 0.5-inch, 0.5-mm-thick silicon wafer was placed on a sample stage as the etched material. After being etched with the above-mentioned CF4 plasma for 1 hour, the thickness distribution of the silicon wafer was measured to evaluate the etching non-uniformity.
[0079] If the plasma etching electrode lacks flatness (i.e., the arithmetic mean waviness is large), the plasma of uniform intensity will not be generated, so even if the etching time is the same, the etching rate of the etched material will be different. Therefore, the smaller the thickness difference of the silicon wafer, the more it indicates that the plasma with uniform intensity is generated.
[0080] Table 2 shows the evaluation results of the arithmetic mean waviness Wa (0 to 10 mm), Wa (10 to 20 mm), Wa (20 to 30 mm) and etching unevenness of each example.
[0081] Before and after plasma etching, the thickness of the silicon wafer at any 17 locations on the etched surface was measured, and the difference in the etching amount on the etched surface was evaluated. Here, the evaluation index is the value of "minimum etching amount / maximum etching amount". If the value is 0.98 or more, it is judged to be better than the prior art (A); if it is 0.95 or more and less than 0.98, it is judged to be the same as the prior art (B); if it is less than 0.95, it is judged to be worse than the prior art (C).
[0082] (Volume resistivity evaluation method)
[0083] The volume resistivity of the polycrystalline SiC film is measured by the four-probe method. The measurement sites are the center point of one main surface of the polycrystalline SiC film and any other 9 points. Here, the volume resistivity of the polycrystalline SiC film is the arithmetic mean of the measured values of the above 10 points, and the deviation of the volume resistivity is evaluated by the standard deviation.
[0084] (Evaluation results and inspection)
[0085] Comparative Example 1 only used a porous holder to fix the polycrystalline SiC film and polished it. At this time, the values of all arithmetic mean waviness in the three wavelength ranges were greater than those of Examples 1 to 3. It can be seen that the polishing method using only a porous holder for fixing cannot remove the waviness on the main surface. In addition, when etching was performed using a plasma etching electrode made of the polycrystalline SiC film of Comparative Example 1, etching unevenness was greater than that of Examples 1 to 3.
[0086] In Examples 1 to 3, the values of all arithmetic mean waviness in the three wavelength ranges are smaller than those in Comparative Examples 1 to 5, the etching non-uniformity is small, and the quality is good. Compared with Comparative Example 5, it can be seen that as the steps proceed, the high-frequency ripple removal effect is improved by increasing the Mooney viscosity. The fixing materials with different Mooney viscosities will undergo elastic deformation and fix the polycrystalline SiC film with the vibration of the grinding device generated during the grinding process and the slight deviation of the device alignment, thereby achieving a stronger ripple removal effect than before.
[0087] Here, in Examples 1 to 3 and Comparative Examples 1 to 5, the volume resistivity was less than 0.010 Ωcm. In addition, the standard deviations thereof were less than 0.010.
[0088]
Table 1
[0089]
[0090]
[0091]
Table 2
[0092]
Claims
1. A polycrystalline SiC molded body, the polycrystalline SiC molded body being a film having two opposing main surfaces, in, The two main surfaces include a first main surface and a second main surface, Regarding the arithmetic mean waviness Wa corresponding to the prescribed wavelength range extracted from the cross-sectional curve of the first main surface and the arithmetic mean waviness Wa corresponding to the prescribed wavelength range extracted from the cross-sectional curve of the second main surface, respectively, When the wavelength range is 0 to 10 mm, the Wa is greater than 0.04 μm and less than 0.05 μm; When the wavelength range is 10 to 20 mm, Wa is greater than 0.06 μm and less than 0.13 μm; and, When the wavelength range is 20 to 30 mm, the Wa is greater than or equal to 0.08 μm and less than or equal to 0.20 μm.
2. The polycrystalline SiC molded body according to claim 1, in, The volume resistivity is 0.050 Ωcm or less. The polycrystalline SiC molded body according to claim 1 , which is used as an electrode in a plasma etching device.
4. A method for producing a polycrystalline SiC molded body, wherein the polycrystalline SiC molded body is a polycrystalline SiC molded body according to any one of claims 1 to 3, wherein the method include: a step of forming a polycrystalline SiC film having a main surface; as well as, a step of grinding a main surface of the polycrystalline SiC film, Wherein, the grinding step comprises: A step of grinding the main surface by a first grinding material; After the step of grinding with the first grinding material, a step of grinding the main surface with a second grinding material; and After the step of grinding with the second grinding material, the step of grinding the main surface with a third grinding material, The particle size of the first grinding material is coarser than that of the second grinding material, The second abrasive material has a coarser particle size than the third abrasive material.
5. The method for producing a polycrystalline SiC molded body according to claim 4, in, The step of polishing with the first polishing material includes the step of fixing the polycrystalline SiC film on a supporting substrate using a first fixing material, The step of polishing with the second polishing material includes the step of fixing the polycrystalline SiC film on the support substrate using a second fixing material, The step of polishing with the third polishing material includes the step of fixing the polycrystalline SiC film on the support substrate using a third fixing material, The Mooney viscosity of the first fixing material is less than the Mooney viscosity of the second fixing material, The Mooney viscosity of the second fixing material is lower than the Mooney viscosity of the third fixing material.
6. A plasma etching method, include: The step of manufacturing the polycrystalline SiC molded body using the method according to claim 4 or 5; as well as, The step of plasma etching is performed using the polycrystalline SiC molded body as an electrode.