A wide frequency stable lead-free ferroelectric energy storage ceramic material and preparation method thereof

By introducing Ca0.5TiO3 and Sr2+ doping into Bi0.5Na0.5TiO3 and using the solid-phase sintering method, the problem of insufficient energy storage density and frequency stability of Bi0.5Na0.5TiO3-based materials has been solved, and high-efficiency energy storage density has been achieved. Preparation of lead-free ferroelectric ceramic materials with wide frequency stability, suitable for new energy electric vehicles and other fields.

CN116675530BInactive Publication Date: 2024-10-29SHIHEZI UNIVERSITY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310661192.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-06
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The Bi0.5Na0.5TiO3-based material in the existing ceramic dielectric has excessive residual polarization, resulting in low energy storage density and energy storage efficiency, and insufficient frequency stability, making it difficult to meet the needs of wide-frequency applications.

Method used

Introducing the Ca0.5TiO3 component, using Sr2+ doped Bi0.5Na0.5TiO3, and using solid phase sintering method, combined with wet ball milling and powder pressing technology, a wide frequency and stable lead-free ferroelectric energy storage ceramic material is prepared. Optimize its energy storage performance and frequency stability.

Benefits of technology

It significantly increases the breakdown field strength of the material, reduces the residual polarization intensity, improves the energy storage density and energy storage efficiency, and ensures that the energy storage efficiency fluctuation is less than 5% in the frequency range of 20Hz-250Hz, making it suitable for wide frequency applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116675530B_ABST
    Figure CN116675530B_ABST
Patent Text Reader

Abstract

The invention discloses a wide frequency stable lead-free ferroelectric energy storage ceramic material and a preparation method thereof in the field of functional ceramic material technology. The general chemical composition formula is (1-x)Bi 0.46 Sr 0.06 Na 0.5 TiO3-xCaTiO3, where 0.06≤x≤0.12; the subscript numbers in the general formula represent the molar ratio of the elements. 2+ Bi-doped 0.5 Na 0.5 TiO3 is the modified object, and Ca is introduced 0.5 The TiO3 component adopts the solid phase sintering method to improve its energy storage performance and wide frequency stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of functional ceramic materials, and in particular relates to a wide-frequency stable lead-free ferroelectric energy storage ceramic material and a preparation method thereof. Background Art

[0002] Energy storage ceramic capacitors have the characteristics of high power density, fast charging and discharging speed, high number of cycles, slow attenuation speed, and wide applicable working environment. They meet the needs of energy storage in the new development stage and are widely used in power electronics industries such as new energy electric vehicles, mobile consumer electronics products, small medical devices, and electric pulse weapons. They have large market demand and broad prospects for large-scale industrialization, and therefore have attracted widespread attention and research.

[0003] Ceramic-based dielectric energy storage materials have the characteristics of small size, high energy density, stable operation at high and low temperatures, fast charging and discharging, and wide frequency application. At present, the mainstream performance optimization methods are ion doping, multiphase solid solution, and preparation process improvement.

[0004] For example, the Chinese patent, publication number: CN112174664B, discloses a high energy storage, high efficiency sodium niobate-based ceramic material with a composition formula of (1-x)[0.9 NaNbO3-0.1Bi(Mg 2 / 3 Ta 1 / 3 )O3]-x(Bi 0.5 Na 0.5 ) 0.7 Sr 0.3 TiO3, x is a molar percentage, 0≤x≤0.40, the present invention also discloses a method for preparing a sodium niobate-based ceramic material, including the sodium niobate-based ceramic material with high energy storage and high efficiency, and also includes the following steps: preparing sodium niobate-based ceramic powder; placing the sodium niobate-based ceramic powder into a ball mill for predetermined treatment, and then pressing the product into a green body for pre-sintering; after the pre-sintering is completed, pouring the product into the ball mill for predetermined treatment again, and after the pre-sintering is completed, pressing the powder into a disc with a mold; sintering the disc in a muffle furnace according to sintering conditions to prepare the sodium niobate-based ceramic material, by introducing a strong ferroelectric Bi(Mg 2 / 3 Ta 1 / 3 )O3 and (Bi 0.5 Na 0.5 ) 0.7 Sr 0.3 TiO3 and NaNbO3 antiferroelectric form a uniform solid solution to increase the maximum polarization strength and breakdown field strength of the ceramic material, thereby improving the energy storage density of the dielectric ceramic material.

[0005] However, in actual use, sodium bismuth titanate (Bi 0.5 Na 0.5 TiO3) is a typical relaxor ferroelectric-based material.3+ and Pb 2+ It is an element in the same period, with similar lone pair electrons 6S 2 Configuration, showing strong ferroelectricity and high saturation polarization at room temperature, has high potential for energy storage applications. 0.5 Na 0.5 TiO3 has a high residual polarization intensity, so its energy storage density and efficiency are low. 0.5 Na 0.5 The large residual polarization disadvantage of TiO3-based materials and the improvement of the energy storage performance and frequency stability of ceramic dielectric energy storage materials are solved by the present invention. A wide-frequency stable lead-free ferroelectric energy storage ceramic material and a preparation method are provided to solve the above problems. Summary of the invention

[0006] The present invention proposes a wide frequency stable lead-free ferroelectric energy storage ceramic material and a preparation method thereof. 2+ Bi-doped 0.5 Na 0.5 TiO3 is the modified object, and Ca is introduced 0.5 The TiO3 component adopts the solid phase sintering method to improve its energy storage performance and wide frequency stability.

[0007] In order to achieve the above-mentioned purpose, the technical scheme of the present invention is as follows: a wide frequency stable lead-free ferroelectric energy storage ceramic material, the chemical composition formula is (1-x)Bi 0.46 Sr 0.06 Na 0.5 TiO3-xCaTiO3, wherein 0.06≤x≤0.12; the subscript numbers in the general formula represent the molar ratio of the elements.

[0008] A method for preparing a wide-frequency stable lead-free ferroelectric energy storage ceramic material comprises the following steps:

[0009] Step 1: Weigh the raw materials and calculate (1-x)Bi 0.46 Sr 0.06 Na 0.5 The molar ratio of the TiO3-xCaTiO3 formula components was calculated, and high-purity dry Bi2O3, Na2CO3, SrCO3, CaTiO3 and TiO2 raw material powders were weighed;

[0010] Step 2: ball milling and drying: the mixed material in step 1 is ball milled on a planetary ball mill, and then taken out and dried in a drying oven at 80°C;

[0011] Step 3: Pre-sintering: the powder obtained in step 2 is sieved and crushed, and then placed in an alumina crucible, which is sealed with a cover, and pre-sintered in a muffle furnace at 750-800°C. The pre-sintering holding time is 3 hours;

[0012] Step 4: Granulation and tableting: add 5wt% polyvinyl alcohol to the pre-sintered powder in step 3, the added amount is 6%-7%, mix evenly without agglomeration, and use a powder tablet press to obtain a green body;

[0013] Step 5: high temperature sintering, the green body obtained in step 4 is kept at 500°C for 30 minutes, the ceramic body is obtained after debinding, high temperature sintering, and after sintering, it is cooled to room temperature with the furnace to obtain a wide frequency stable lead-free ferroelectric energy storage ceramic material. Furthermore, the ball milling in step 2 is wet ball milling, and the medium used is anhydrous ethanol; the ball milling time is 12-24 hours.

[0014] Further, the method of using the final tablet press in step 4 is: dry-pressing the powder without lumps at 30 MPa.

[0015] Furthermore, the sintering temperature in step five is 1100-1150° C., and the holding time is 3 hours.

[0016] Furthermore, the heating rate during sintering in step five is 4-8°C / min.

[0017] Furthermore, when the wide-frequency stable lead-free ferroelectric energy storage ceramic material is used as an energy storage capacitor, it is necessary to burn-plate electrodes on the surface of the ceramic body.

[0018] Furthermore, the method of firing and plating the electrode is: coating the surface of the ceramic body with a standard area of ​​silver paste, and then firing at 550-600° C. for 30 minutes.

[0019] The following beneficial effects are achieved by adopting the above scheme:

[0020] 1. The present invention introduces Ca in the component design process 2+ , whose ionic radius is 1.34Å, smaller than that of Bi 3+ The ionic radius (1.38Å) refines the domain structure of the relaxor ferroelectric, increases the breakdown field strength, and reduces the residual polarization strength. Its energy storage performance has been greatly improved compared with existing products. At room temperature and an applied electric field of 260KV / cm, the energy storage density W rec 3.52 J / cm 3 , the energy storage efficiency is 73.3%.

[0021] 2. The preparation method of the present invention is simple and has good repeatability. The obtained ceramic material has a wide frequency stability and maintains an energy storage efficiency fluctuation of less than 5% within the frequency range of 20Hz-250Hz. It is highly practical and has good application prospects in the field of pulse power materials.

[0022] 3. The medium used in wet ball milling is anhydrous ethanol, because anhydrous ethanol can provide better dispersing properties, which helps to maintain the dispersion state of powder particles and avoid powder agglomeration during ball milling. Compared with water, anhydrous ethanol has a lower boiling point, which is conducive to the rapid dissipation of heat generated during ball milling, thereby effectively controlling the temperature rise of ball milling. Anhydrous ethanol has high chemical stability and is not prone to oxidation reactions and metal ion contamination, which can ensure product purity. The use of anhydrous ethanol can also control the pH value during ball milling, further optimizing the powder preparation process.

[0023] 4. Green embryo production: Use a powder tablet press to dry-press the non-agglomerated powder at 30MPa. This method can produce green embryos with uniform density and uniform particle size. High-quality green embryos provide a reliable foundation for subsequent material preparation. The powder tablet press has a high degree of automation and can prepare green embryos in large quantities, which improves production efficiency. The wet preparation process needs to consider the interaction between particles and solution, which is relatively complicated, but dry pressing can simplify this process, making it easier to control the quality of the green embryos.

[0024] 5. Silver paste is coated on the surface of the ceramic body, forming a good chemical bond between silver and the material, which can improve the bonding strength between the electrode and the material; during the firing and plating process, the silver paste and the ceramic body can be fully fired and plated together, making the electrode surface smooth and uniform, which is beneficial to the performance stability of the capacitor; the firing and plating temperature is moderate and the time is short, which will not cause changes in the internal structure of the ceramic body, thereby ensuring the stability and reliability of the ceramic body; the excellent conductive properties of the silver paste can effectively improve the electrode conductivity of the ceramic body and improve the performance parameters of the ceramic body. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the XRD diagram of the ceramic body prepared in Examples 2-5 of the wide-frequency stable lead-free ferroelectric energy storage ceramic material and preparation method of the present invention.

[0026] Figure 2 This is a SEM image of the ceramic embryo prepared in Examples 2-5 of the wide-frequency stable lead-free ferroelectric energy storage ceramic material and preparation method of the present invention.

[0027] Figure 3 This is a bipolar PE hysteresis loop diagram of the ceramic body prepared in Example 4 of the wide-frequency stable lead-free ferroelectric energy storage ceramic material and preparation method of the present invention.

[0028] Figure 4 This is a bipolar PE hysteresis loop diagram of the ceramic body prepared in Example 5 of the wide-frequency stable lead-free ferroelectric energy storage ceramic material and preparation method of the present invention.

[0029] Figure 5This is a frequency stability PE hysteresis loop diagram of the ceramic embryo prepared in Example 4 of the wide-frequency stable lead-free ferroelectric energy storage ceramic material and preparation method of the present invention.

[0030] Figure 6 This is an underdamped pulse discharge diagram of a ceramic body prepared in Example 4 of the wide-frequency stable lead-free ferroelectric energy storage ceramic material and preparation method of the present invention. DETAILED DESCRIPTION

[0031] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0032] In the description of the present invention, it is to be understood that the terms “longitudinal”, “lateral”, “vertical”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside” and “outside” etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0033] In the description of the present invention, unless otherwise specified and limited, it should be noted that the terms "installed", "connected" and "connected" should be understood in a broad sense. For example, it can be a mechanical connection or an electrical connection, or it can be the internal connection between two components. It can be a direct connection or an indirect connection through an intermediate medium. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to the specific circumstances.

[0034] The following is further described in detail through specific implementation methods:

[0035] Embodiment 1, basically as attached Figure 1-6 As shown: A wide frequency stable lead-free ferroelectric energy storage ceramic material, the raw material powders and purity used are: Bi2O3 (99.9%), Na2CO3 (99.5%), SrCO3 (99.95%), CaTiO3 (99.5%) and TiO2 (99%), all purchased from the official website of Aladdin Reagent. The energy density and energy efficiency data involved in this embodiment are all calculated from the polarization-electric field intensity (PE) curve measured by the Agilent ferroelectric comprehensive analyzer in the United States.

[0036] Example 2 is different from the above example in that the chemical composition is 0.94Bi 023 r 0.06Na 0.5 The formula of TiO3-0.06CaTiO3 is to weigh the raw materials in molar proportion, perform planetary ball milling for 24 hours, and after drying, pre-sinter the powder in an alumina crucible at 800°C for 3 hours and naturally cool to room temperature; the pre-sintered powder is ball-milled again for 24 hours, pressed into tablets after drying, and the pressed embryo is sintered in a muffle furnace, kept at 500°C for 30 minutes to debind, and then heated to 1150°C at 4°C / min and kept for 3 hours. After sintering, it is cooled to room temperature with the furnace to obtain a wide-frequency stable lead-free ferroelectric energy storage ceramic embryo.

[0037] Example 3 is different from the above examples in that the chemical composition is 0.92Bi 0.46 Sr 0.06 Na 0.5 The formula of TiO3-0.08CaTiO3 is to weigh the raw materials in molar proportion, perform planetary ball milling for 24 hours, and after drying, pre-sinter the powder in an alumina crucible at 800°C for 3 hours and naturally cool to room temperature; the pre-sintered powder is ball milled again for 24 hours, pressed into tablets after drying, and the pressed embryo is sintered in a muffle furnace, kept at 500°C for 30 minutes to debind, and then heated to 1150°C at 4°C / min and kept for 3 hours. After sintering, it is cooled to room temperature with the furnace to obtain a wide-frequency stable lead-free ferroelectric energy storage ceramic embryo.

[0038] Example 4 is different from the above examples in that the chemical composition is 0.90Bi 0.46 Sr 0.06 Na 0.5 The formula of TiO3-0.10CaTiO3 is to weigh the raw materials in molar proportion, perform planetary ball milling for 24 hours, and after drying, pre-sinter the powder in an alumina crucible at 800°C for 3 hours and naturally cool to room temperature; the pre-sintered powder is ball milled again for 24 hours, pressed into tablets after drying, and the pressed embryo is sintered in a muffle furnace, kept at 500°C for 30 minutes to debind, and then heated to 1150°C at 4°C / min and kept for 3 hours. After sintering, it is cooled to room temperature with the furnace to obtain a wide-frequency stable lead-free ferroelectric energy storage ceramic embryo.

[0039] Example 5 is different from the above examples in that the chemical composition is 0.88Bi 0.46 Sr 0.06 Na 0.5The formula of TiO3-0.12CaTiO3 is to weigh the raw materials in molar proportion, perform planetary ball milling for 24 hours, and after drying, pre-sinter the powder in an alumina crucible at 800°C for 3 hours and naturally cool to room temperature; the pre-sintered powder is ball milled again for 24 hours, pressed into tablets after drying, and the pressed embryo is sintered in a muffle furnace, kept at 500°C for 30 minutes to debind, and then heated to 1150°C at 4°C / min and kept for 3 hours. After sintering, it is cooled to room temperature with the furnace to obtain a wide-frequency stable lead-free ferroelectric energy storage ceramic embryo.

[0040] The specific implementation process is as follows: select one ceramic body prepared in Examples 2-5, polish the surface with 240 mesh corundum and water, polish to 1 mm, clean with ultrasonic wave and dry. XRD test is performed with X-ray diffractometer (Bruker D8Advance), and the results are shown in Figure 1 .

[0041] Depend on Figure 1 It can be seen that the ceramic body is a single-phase perovskite structure, and no obvious second-phase impurities are found. 2+ and Ca 2+ Diffusion into the crystal lattice to form a solid solution.

[0042] One ceramic body prepared in Examples 2-5 was selected from each of them, and the surface was polished to 1 mm using 240 mesh corundum and water, and then cleaned by ultrasonic cleaning and dried. The surface SEM image was measured using a scanning electron microscope (SU8010, Hitachi, Japan). The results are shown in Figure 2 .

[0043] Depend on Figure 2 It can be seen that as the component CaTiO3 is added, the grain size is reduced, which helps to improve the ferroelectricity of the material.

[0044] One ceramic body prepared in each of Examples 4 and 5 was selected, and the surface was polished with 240 mesh, 600 mesh, and 1500 mesh corundum and water in turn until the surface was polished to 0.16 mm. The ceramic body was cleaned with ultrasonic wave and then dried. A silver electrode with a diameter of 1 mm was applied on the ceramic surface, and the lower surface was completely covered with the silver electrode. The ceramic body was placed in a muffle furnace at 550° C. for 30 min, and naturally cooled to room temperature. The bipolar PE hysteresis loop was measured using a ferroelectric analysis system (LC II-100V, Radiant, USA). The results are shown in FIG. Figure 3-4 .

[0045] Depend on Figure 3 It can be seen that with the increase of the external electric field, the energy storage density W at room temperature and 260KV / cm external electric field is rec 3.52 J / cm 3 , the energy storage efficiency is 73.3%.

[0046] Depend on Figure 4 It can be seen that under the maximum applied electric field strength of 250KV / cm, the energy storage density W is obtained. rec 3.27J / cm 3 , the energy storage efficiency is 80.0%.

[0047] One ceramic body prepared in Example 4 was selected, and the surface was polished with 240 mesh, 600 mesh, and 1500 mesh corundum and water, polished to 0.16 mm, cleaned with ultrasonic wave, and dried. A silver electrode with a diameter of 1 mm was applied to the ceramic surface, and the lower surface was completely covered with the silver electrode. It was placed in a muffle furnace at 550°C for 30 minutes, cooled naturally to room temperature, and the frequency stability of the bipolar PE hysteresis loop was measured using a ferroelectric analysis system (LC II-100V, Radiant, USA). The test results are shown in Figure 5 .

[0048] Depend on Figure 5 It can be seen that within a wider frequency range, the ceramic body of Example 4 still maintains a good hysteresis loop without obvious deformation, and the energy storage efficiency fluctuation is <5%, indicating that within the frequency range of 20-250Hz, the ceramic body has excellent frequency stability.

[0049] One ceramic body prepared in Example 4 was selected, and its surface was polished with 240 mesh, 600 mesh, and 1500 mesh corundum and water in turn until it was polished to 0.16 mm. It was cleaned with ultrasonic wave and dried. A silver electrode with a diameter of 1 mm was applied on the ceramic surface, and the lower surface was completely covered with the silver electrode. The ceramic body was placed in a muffle furnace at 550° C. for 30 min, and naturally cooled to room temperature. The charge and discharge performance of the sample was tested using a capacitive charge and discharge system (CDTS-10, JYJS Technology Co., China). The test results are shown in FIG. Figure 6 .

[0050] Depend on Figure 6 It can be seen that the ceramic body of Example 4 has a higher current density CD of 349.58A / cm 2 The maximum power density PD is 18.90MW / cm 3 charge and discharge performance.

[0051] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and / or characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A wide frequency stable lead-free ferroelectric energy storage ceramic material, characterized by: The general chemical formula is (1-x)Bi 0.46 Sr 0.06 Na 0.5 TiO3-xCaTiO3, wherein 0.06≤x≤0.12; the subscript numbers in the general formula represent the molar ratio of the elements.

2. A method for preparing a wide frequency stable lead-free ferroelectric energy storage ceramic material, characterized in that: The method for preparing the wide-frequency stable lead-free ferroelectric energy storage ceramic material according to claim 1 comprises the following steps: Step 1: Weigh the raw materials and calculate (1-x)Bi 0.46 Sr 0.06 Na 0.5 The molar ratio of the TiO3-xCaTiO3 formula components was calculated, and high-purity dry Bi2O3, Na2CO3, SrCO3, CaTiO3 and TiO2 raw material powders were weighed; Step 2: ball milling and drying: the mixed material in step 1 is ball milled on a planetary ball mill, and then taken out and dried in a drying oven at 80°C; Step 3: Pre-sintering: the powder obtained in step 2 is sieved and crushed, and then placed in an alumina crucible, which is sealed with a cover, and pre-sintered in a muffle furnace at 750-800°C. The pre-sintering holding time is 3 hours; Step 4: Granulation and tableting: add 5wt% polyvinyl alcohol to the pre-sintered powder in step 3, the added amount is 6%-7%, mix evenly without agglomeration, and use a powder tablet press to obtain a green body; Step 5: high temperature sintering, the green body obtained in step 4 is kept at 500°C for 30 minutes, the ceramic body is obtained after debinding, and high temperature sintering is performed. After sintering, it is cooled to room temperature with the furnace to obtain a wide frequency stable lead-free ferroelectric energy storage ceramic material.

3. The method for preparing the wide frequency stable lead-free ferroelectric energy storage ceramic material according to claim 2, characterized in that: The ball milling in step 2 is wet ball milling, and the medium used is anhydrous ethanol; the ball milling time is 12-24h.

4. The method for preparing the wide frequency stable lead-free ferroelectric energy storage ceramic material according to claim 3, characterized in that: Method of using the powder tablet press in step 4: dry-press the non-agglomerated powder at 30 MPa.

5. The method for preparing the wide frequency stable lead-free ferroelectric energy storage ceramic material according to claim 4, characterized in that: The sintering temperature in step 5 is 1100-1150°C, and the holding time is 3h.

6. The method for preparing the wide frequency stable lead-free ferroelectric energy storage ceramic material according to claim 5, characterized in that: The heating rate during sintering in step five is 4-8°C / min.

7. The method for preparing a wide frequency stable lead-free ferroelectric energy storage ceramic material according to claim 6, characterized in that: When the wide-frequency stable lead-free ferroelectric energy storage ceramic material is used as an energy storage capacitor, it is necessary to burn-plate electrodes on the surface of the wide-frequency stable lead-free ferroelectric energy storage ceramic material.

8. The method for preparing a wide frequency stable lead-free ferroelectric energy storage ceramic material according to claim 7, characterized in that: The method of firing and plating electrodes is as follows: coating the surface of the wide-frequency stable lead-free ferroelectric energy storage ceramic material with a standard area of ​​silver paste, and then firing at 550-600°C for 30 minutes.

Citation Information

Patent Citations

  • A high-energy-storage, high-efficiency sodium niobate-based ceramic material and its preparation method

    CN112174664B