Mobile phone protective film UV matte ink and preparation method thereof

By combining modified epoxy acrylic resin with polyester resin and the use of polysiloxane-polyether copolymer, combined with modified polyethylene wax powder and photoinitiator, a dense crosslinking network structure is formed, and UV matte is solved The problem of ink volume reduction and insufficient wear resistance has achieved the ideal matte effect and wear resistance of ink.

CN116676016BActive Publication Date: 2024-11-15SHENZHEN ALTO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310793481.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-30
Publication Date
2024-11-15
Estimated Expiration
2043-06-30

AI Technical Summary

Technical Problem

The existing UV matte inks shrinks in volume during curing, resulting in exposure of inorganic fillers, making it difficult to form an ideal matte effect, and lack of wear resistance.

Method used

Modified epoxy acrylic resin and polyester resin are blended with polysiloxane-polyether copolymer and modified polyethylene wax powder to form a dense crosslinking network structure, which prompts the inorganic filler to migrate to the surface layer and aggregate to form a dumb Light effect and improve friction resistance through photoinitiators.

Benefits of technology

It achieves a good matte effect on the ink surface and improves friction resistance, and enhances the dispersion and wear resistance of the inorganic filler.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0005088055140000071
    Figure GDA0005088055140000071
  • Figure GDA0005088055140000072
    Figure GDA0005088055140000072
  • Figure GDA0005088055140000081
    Figure GDA0005088055140000081
Patent Text Reader

Abstract

The present application relates to the field of printing inks, and specifically discloses a UV matte ink for a mobile phone protective film and a preparation method thereof. A UV matte ink for a mobile phone protective film comprises the following raw materials in parts by weight: 40-50 parts of modified epoxy acrylic resin, 0.5-2 parts of polysiloxane-polyether copolymer, 40-50 parts of polyester resin, 20-30 parts of reactive diluent, 20-30 parts of photoinitiator, 3-5 parts of colorant, 3-10 parts of inorganic filler, and 5-10 parts of modified polyethylene wax powder; its preparation method is: after the modified polyethylene wax powder is mixed and ground with the inorganic filler, it is fully mixed with other ingredients, and ultrasonic dispersion is used to fully mix the components to obtain a UV matte ink for a mobile phone protective film. The composition of the present application can be used for printing on a mobile phone protective film, and it has the advantage of good friction resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of printing inks, and more specifically, to a UV matte ink for a mobile phone protective film and a preparation method thereof. Background Art

[0002] UV curing ink is a new type of ink popular in Europe, America, Japan and other places at the end of the 20th century. It was first used in the surface coating of furniture, floors, mobile phones, and Walkman shells. Its application field has now been further expanded to cosmetic containers, household appliances such as televisions and computers, and other fields such as motorcycles and glazing. UV curing ink has the advantages of not containing volatile organic compounds (VOC), less pollution to the environment, fast curing speed, energy saving, good performance of the cured product, and suitable for high-speed automated production. Traditional inks are volatile and slow to cure, which is not conducive to environmental protection. Therefore, UV ink is the main substitute for traditional inks.

[0003] UV matte ink for mobile phone protective film is a special coating technology that can form a uniform matte coating on the surface of the mobile phone protective film, making the mobile phone screen clearer and less susceptible to fingerprints and dirt, while also effectively preventing screen scratches and damage. UV matte ink is a fast-curing coating that dries and hardens quickly through ultraviolet radiation, and has the characteristics of high strength, high wear resistance and high transparency.

[0004] UV (ultraviolet curing) ink refers to an ink that uses ultraviolet light of different wavelengths and energies to polymerize the monomers in the ink binder into polymers under ultraviolet light, so that the ink forms a film and dries. The composition of UV matte ink is very different from that of traditional ink. The film formation of UV matte ink is a chemical reaction, and the monomers and polymers undergo polymerization under the action of initiators, while the film formation of traditional matte ink is a physical action. The resin is already a polymer, and the solvent dissolves the solid polymer into a liquid polymer. After printing on the substrate, as a large amount of solvent evaporates, the volume of the ink film is bound to shrink significantly (the film thickness can lose as much as 60%), and the inorganic particles in the film are easily exposed on the surface of the dry film, which not only achieves a matte effect, but also enhances the sand feeling. The liquid polymer returns to its original solid state, forming a matte effect attached to the surface of the object. UV curing inks contain basically no volatile components, and the film-forming and curing principle is completely different from that of solvent-based inks. They can be dried and cured within seconds, there is no large amount of solvent volatilization, and the volume of the ink film will not shrink significantly, making it difficult for inorganic filler particles to be exposed on the surface of the ink film, and it is difficult to form a concave and convex surface, so the matte effect is not strong.

[0005] Usually, adding micro powder wax or inorganic matte powder to UV curing ink can produce a matte effect. Wax is a very common component in ink, which is used to change the rheology of ink, improve water resistance and printing performance, and make the printed dots uniform and complete. This matte effect has a soft feel and waxy texture, but because the wax powder only floats on the surface of the printed film, and the wax itself has low strength and poor scratch resistance, the effect is mostly not ideal. If inorganic filler components such as fumed silica, silica powder, talcum powder, etc. are added instead, it will be difficult to obtain a matte effect due to their poor adhesion to the surface of the film layer. Summary of the invention

[0006] In order to improve the wear resistance of matte ink, the present application provides a mobile phone protective film UV matte ink and a preparation method thereof.

[0007] In the first aspect, the present application provides a mobile phone protective film UV matte ink, which adopts the following technical solution:

[0008] A mobile phone protective film UV matte ink, comprising the following raw materials in parts by weight:

[0009] 40-50 parts of modified epoxy acrylic resin, 0.5-2 parts of polysiloxane-polyether copolymer, 40-50 parts of polyester resin, 20-30 parts of active diluent, 20-30 parts of photoinitiator, 3-5 parts of colorant, 3-10 parts of inorganic filler, and 5-10 parts of modified polyethylene wax powder.

[0010] By adopting the above technical solution, modified epoxy acrylic resin and polyester resin are blended, that is, the UV cationic system and UV free radicals are mixed, the inhibition of oxygen in the air on the photocuring of the resin is reduced, and a dense cross-linked network structure is formed with a multi-functional active diluent with double bonds under the initiation of the photoinitiator, thereby improving the friction resistance of the ink. The incomplete compatibility of the inorganic filler and the organic cross-linked network forces the inorganic particles to migrate to the surface layer with poor curing conditions and gather on the surface of the ink layer. The polysiloxane-polyether copolymer gives the ink good rheological properties and settles during solidification, thereby achieving a better matte effect on the ink surface. The active diluent has multiple functional groups. In theory, a small active diluent molecule has 4 double bonds, which can better promote polymerization and cross-linking during photocuring. Polysiloxane-polyether copolymer and modified polyethylene wax powder have excellent slip-enhancing effect, and can also improve scratch resistance, form a dense silicone layer on the surface of the ink film, improve the friction resistance of the ink, and can be wrapped on inorganic filler powder to increase the matte effect, thereby improving the dispersibility of the inorganic filler.

[0011] Optionally, the modified epoxy acrylic resin is modified with hydroxyethyl methacrylate.

[0012] By adopting the above technical solution, hydroxyethyl methacrylate is a monomer containing double bonds and hydroxyl groups, which can react with epoxy groups in epoxy acrylic resin to form a cross-linked structure, thereby improving the mechanical properties and chemical resistance of epoxy resin. In addition, hydroxyethyl methacrylate can also enhance the compatibility and adhesion of the resin by hydrogen bonding or electrostatic interaction with carboxyl or amide groups in the resin through the hydroxyl group.

[0013] Optionally, the preparation method of the modified epoxy acrylic resin is as follows:

[0014] The preparation method of the modified epoxy acrylic resin is as follows:

[0015] (1) Mix epoxy resin and acrylic acid and heat to 70-80°C, slowly add dimethylaniline and azobisisobutyronitrile and heat to 80-110°C, keep warm for reaction, terminate the reaction when the acid value is lower than 6 mgKOH / g, cool naturally to obtain epoxy acrylic resin; (2) Evenly mix the epoxy acrylic resin obtained above with hydroxyethyl methacrylate, triethylamine and dimethylaniline, heat to 60-80°C for reaction for 15-20h, precipitate with ether 3 times, and dry to obtain epoxy resin modified with hydroxyethyl methacrylate.

[0016] By adopting the above technical scheme, an epoxy acrylic resin modified by ethyl methacrylate is prepared. Under the action of an initiator and an auxiliary agent, the epoxy resin undergoes a ring-opening reaction with acrylic acid to obtain an epoxy acrylic resin, which is then mixed with ethyl methacrylate to obtain a modified epoxy acrylic resin.

[0017] Optionally, the epoxy resin is an aliphatic epoxy resin.

[0018] By adopting the above technical solution, considering the photoactivity of the resin, it must have deep curing ability to ensure that the bottom layer is cured first during curing, and at the same time have a certain stable synergistic photosensitization effect. It is more appropriate to use aliphatic epoxy resin.

[0019] Optionally, the modified polyethylene wax powder is obtained by modifying polytetrafluoroethylene.

[0020] By adopting the above technical scheme, the polyethylene wax powder modified with polytetrafluoroethylene has good friction resistance. At the same time, because the polyethylene wax powder has low density and good dispersibility, it is easy to disperse in the ink, and the inorganic filler is wrapped and evenly dispersed in the resin. When solidifying into a film, it is incompatible with the resin system and floats on the surface of the solidified ink film, thereby reducing the gloss, matting and increasing the slip, and improving the friction resistance.

[0021] Optionally, the photoinitiator is a cationic photoinitiator, which is one of iodonium salt, sulfonium salt and iron arene.

[0022] By adopting the above technical scheme, the photoinitiator is activated by ultraviolet light to bring the molecules to an excited state. The molecules undergo a series of cracking reactions to produce Lewis strong acids, which act as active sites to carry out a ring-opening reaction of the epoxy resin, generate active free radicals, and initiate cationic photopolymerization reactions while initiating free radical polymerization. The curing shrinkage rate of the resin is greater than that of a single cationic photopolymerization initiator, which is beneficial to the emergence of inorganic fillers, ensures the matte effect of the ink, and improves the abrasion resistance of the ink.

[0023] Optionally, the powder filler is a mixture of talcum powder and any one of quartz powder and ceramic powder; the particle size of the talcum powder is 2.5-2.7 μm, the particle size of the quartz powder is 1.3-1.6 μm, and the particle size of the ceramic powder is 4.5-5 μm.

[0024] By adopting the above technical scheme, the matte effect of UV ink is presented by relying on the diffuse reflection principle of matte powder for matte. It is necessary to add enough light-absorbing components to the ink as much as possible to reduce the amount of reflection to ensure the formula is transparent and projective curing, stabilize photons, diffuse reflection and matte, and absorb non-curing light as much as possible. Therefore, when selecting powder fillers, its dispersibility in the system and synergistic matte properties should be considered. Talc with a particle size of 2.5-2.7μm has good synergistic matte and permeability, quartz powder with a particle size of 1.3-1.6μm and ceramic powder with a particle size of 4.5-5μm have good wear resistance. Talc is mixed with quartz powder or ceramic powder to ensure ink permeability while synergistic matte, thereby improving the wear resistance and matte effect of UV ink.

[0025] In the second aspect, the present application provides a method for preparing UV matte ink for a mobile phone protective film, using the following technical solution:

[0026] A method for preparing UV matte ink for a mobile phone protective film, comprising the following preparation steps:

[0027] (1) mixing and grinding the modified polyethylene wax powder and the inorganic filler to obtain a mixed inorganic filler;

[0028] (2) Weighing modified epoxy acrylic resin and polyester resin and dissolving them in water, adding active diluent, photoinitiator, colorant and the mixed inorganic filler in step (1) in turn, and ultrasonicating for 30 minutes to fully mix the components to obtain UV matte ink for mobile phone protective film

[0029] By adopting the above technical scheme, the modified polyethylene wax powder and the inorganic filler are first mixed and ground, and the inorganic filler is fully contacted with the modified polyethylene wax powder and then dispersed and mixed with other ingredients to obtain a finished product, which is simple and convenient to operate.

[0030] In summary, this application has the following beneficial effects:

[0031] 1. Since the present application uses hydroxyethyl methacrylate to modify the epoxy acrylic resin, the hydroxyethyl methacrylate undergoes esterification and cross-linking reaction with the epoxy group and acrylic acid in the epoxy acrylic resin, thereby increasing the molecular weight of the resin, and cross-linking with the polyester resin to form a tight network structure, thereby achieving better friction resistance.

[0032] 2. In this application, polyethylene wax powder modified with polytetrafluoroethylene is preferably used to improve the friction resistance of polyethylene wax powder. At the same time, polyethylene wax powder with good dispersibility wraps inorganic fillers and is evenly dispersed in the ink. When curing, it floats on the surface of the cured ink, thereby reducing the glossiness to obtain a better matte effect while improving the friction resistance of the ink. DETAILED DESCRIPTION

[0033] The present application is further described in detail below in conjunction with embodiments.

[0034] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0035] Polysiloxane polyether copolymer was purchased from Guangzhou Jinkai Chemical Co., Ltd.;

[0036] Preparation examples of raw materials and / or intermediates

[0037] Preparation Example 1

[0038] A modified epoxy acrylic resin, the preparation method is as follows:

[0039] (1) 1 kg of epoxy resin and 1.2 kg of acrylic acid were placed in a flask, mixed and heated to 70° C., 0.5 kg of dimethylaniline and 0.2 kg of azobisisobutyronitrile were slowly added dropwise, the temperature was raised to 80° C., and the reaction was kept at this temperature for 8 hours. When the acid value was 5.9 mgKOH / g, the reaction was terminated, the temperature was naturally lowered, and the epoxy acrylic resin was stored away from light to obtain;

[0040] (2) The epoxy acrylic resin obtained above was mixed evenly with 3.2 kg of hydroxyethyl methacrylate, 2.1 kg of triethylamine, and 0.5 kg of dimethylaniline, and the mixture was heated to 70° C. for reaction for 15 h. Ether precipitation was performed three times, and the mixture was dried to obtain an epoxy resin modified with hydroxyethyl methacrylate.

[0041] Preparation Example 2

[0042] A modified epoxy acrylic resin, the preparation method is as follows:

[0043] (1) 1 kg of epoxy resin and 1.2 kg of acrylic acid were placed in a flask, mixed and heated to 75° C., 0.5 kg of dimethylaniline and 0.2 kg of azobisisobutyronitrile were slowly added dropwise, the temperature was raised to 95° C., and the reaction was kept at this temperature for 8 hours. When the acid value was 5.9 mgKOH / g, the reaction was terminated, the temperature was naturally lowered, and the epoxy acrylic resin was stored away from light to obtain;

[0044] (2) The epoxy acrylic resin obtained above was mixed evenly with 3.2 kg of hydroxyethyl methacrylate, 2.1 kg of triethylamine, and 0.5 kg of dimethylaniline, and the mixture was heated to 60° C. for reaction for 15 h. Ether precipitation was performed three times, and the mixture was dried to obtain an epoxy resin modified with hydroxyethyl methacrylate.

[0045] Preparation Example 3

[0046] A modified epoxy acrylic resin, the preparation method is as follows:

[0047] (1) 1 kg of epoxy resin and 1.2 kg of acrylic acid were placed in a flask, mixed and heated to 80° C., 0.5 kg of dimethylaniline and 0.2 kg of azobisisobutyronitrile were slowly added dropwise, the temperature was raised to 110° C., and the reaction was kept at this temperature for 8 hours. When the acid value was 5.9 mgKOH / g, the reaction was terminated, the temperature was naturally lowered, and the epoxy acrylic resin was stored away from light to obtain;

[0048] (2) The epoxy acrylic resin obtained above was mixed evenly with 3.2 kg of hydroxyethyl methacrylate, 2.1 kg of triethylamine, and 0.5 kg of dimethylaniline, and the mixture was heated to 80° C. for reaction for 15 h. Ether precipitation was performed three times, and the mixture was dried to obtain an epoxy resin modified with hydroxyethyl methacrylate.

[0049] Comparative Preparation Example 1

[0050] A modified epoxy acrylic resin, the preparation method is as follows:

[0051] (1) 1 kg of epoxy resin and 1.2 kg of acrylic acid were placed in a flask, mixed and heated to 80° C., 0.5 kg of dimethylaniline and 0.2 kg of azobisisobutyronitrile were slowly added dropwise, the temperature was raised to 110° C., and the reaction was kept at this temperature for 8 hours. When the acid value was 5.9 mgKOH / g, the reaction was terminated, the temperature was naturally lowered, and the epoxy acrylic resin was stored away from light to obtain;

[0052] (2) The epoxy acrylic resin obtained above was mixed evenly with 3.2 kg of succinic acid, 2.1 kg of triethylamine and 0.5 kg of dimethylaniline, and the mixture was heated to 80° C. for reaction for 15 h. Ether was used for precipitation three times, and the mixture was dried to obtain an epoxy resin modified with hydroxyethyl methacrylate.

[0053] The epoxy resins used in Preparation Examples 1-3 and Comparative Preparation Example 1 are all 4-epoxycyclohexylcarboxylic acid-3,4-epoxycyclohexyl methyl ester.

[0054] Comparative Preparation Example 2

[0055] A modified epoxy acrylic resin is different from Preparation Example 1 in that the epoxy resin used in this comparative preparation example is ordinary bisphenol A epoxy resin.

[0056] Example

[0057] Example 1

[0058] A mobile phone protective film UV matte ink, the preparation method is as follows:

[0059] (1) 50 g of modified polyethylene wax powder, 50 g of talc powder and 50 g of quartz powder were mixed and ground at 1000 r / min for 10 min to obtain a mixed inorganic filler;

[0060] (2) Weigh 400 g of the modified epoxy acrylic resin prepared in Preparation Example 1 and 500 g of the polyester resin and dissolve them in 1 L of water, then add 200 g of 1,6-hexanediol diacrylate, 300 g of diphenyliodonium salt, 50 g of colorant and the mixed inorganic filler obtained in step (1) in turn, mix them evenly and ultrasonicate for 30 min to fully mix the components to obtain UV matte ink for mobile phone protective film.

[0061] Example 2

[0062] A mobile phone protective film UV matte ink, the preparation method is as follows:

[0063] (1) 75 g of modified polyethylene wax powder, 30 g of talc powder and 35 g of quartz powder were mixed and ground at 1000 r / min for 10 min to obtain a mixed inorganic filler;

[0064] (2) Weigh 450 g of the modified epoxy acrylic resin obtained in Preparation Example 2 and 450 g of the polyester resin and dissolve them in 1 L of water. Then add 250 g of 1,6-hexanediol diacrylate, 250 g of diphenyliodonium salt, 30 g of colorant and the mixed inorganic filler obtained in step (1) in turn and mix them by ultrasonication for 30 min to fully mix the components to obtain UV matte ink for mobile phone protective film.

[0065] Example 3

[0066] A mobile phone protective film UV matte ink, the preparation method is as follows:

[0067] (1) 100 g of modified polyethylene wax powder, 15 g of talc powder and 15 g of quartz powder were mixed and ground at 1000 r / min for 10 min to obtain a mixed inorganic filler;

[0068] (2) Weigh 500 g of the modified epoxy acrylic resin prepared in Preparation Example 3 and 400 g of the polyester resin and dissolve them in 1 L of water. Then add 300 g of 1,6-hexanediol diacrylate, 200 g of diphenyliodonium salt, 40 g of colorant and the mixed inorganic filler obtained in step (1) in turn and mix them by ultrasonication for 30 min to fully mix the components to obtain UV matte ink for mobile phone protective film.

[0069] Example 4

[0070] A UV matte ink for a mobile phone protective film, which is different from Example 1 in that the photoinitiator in this example is a triarylsulfonium salt.

[0071] Example 5

[0072] A UV matte ink for a mobile phone protective film, which is different from Example 1 in that the photoinitiator in this example is η6-isopropylphenylferrocene (II) hexafluorophosphate.

[0073] Example 6

[0074] A UV matte ink for a mobile phone protective film, which is different from Example 5 in that the inorganic filler used in this example is a mixture of talcum powder and ceramic powder.

[0075] Comparative Example

[0076] Comparative Example 1

[0077] A UV matte ink for a mobile phone protective film, which is different from Example 1 in that the modified epoxy acrylic resin used in this comparative example is prepared using Comparative Preparation Example 1.

[0078] Comparative Example 2

[0079] A UV matte ink for a mobile phone protective film, which is different from Example 1 in that the modified epoxy acrylic resin used in this comparative example is prepared using Comparative Preparation Example 2.

[0080] Comparative Example 3

[0081] A UV matte ink for a mobile phone protective film, which is different from Example 1 in that unmodified polyethylene wax powder is used in this comparative example.

[0082] Comparative Example 4

[0083] A UV matte ink for a mobile phone protective film, which is different from Example 1 in that the initiator used in this comparative example is a free radical initiator, sodium persulfate.

[0084] Comparative Example 5

[0085] A UV matte ink for a mobile phone protective film, which is different from Example 1 in that a single talcum powder is used as an inorganic filler in this comparative example.

[0086] Performance testing

[0087] Detection Methods

[0088] Abrasion resistance test: First weigh the mass m1 (g) of a square PET protective film with a side length of 1 cm, apply UV ink on the PET protective film and cure it under ultraviolet light, weigh the mass m2 (g), and get the mass of the ink film from m2-m1. Cover the ink film with sandpaper with a particle size of 50μm, place a 500g weight, and continuously drag the sandpaper to make it rub against the ink film. Weigh the mass m3 (g) after 50 times of friction. The mass loss rate of the ink film (w) can be obtained from the following formula to judge the abrasion resistance of the ink. The lower the ink film loss rate, the better the abrasion resistance of the ink;

[0089]

[0090] Gloss: Use German BYK gloss meter, model BYK4561, to read 60° gloss data

[0091] Table 1 Test performance test results

[0092]

[0093]

[0094] Combining Examples 1-3 with Comparative Example 1 and Table 1, it can be seen that the test data of Examples 1-3 are better than those of Comparative Example 1, indicating that the molecular chain of the epoxy acrylic resin modified with hydroxyethyl methacrylate is lengthened, the molecular weight is increased, and it is cross-linked and cured with the polyester resin and the active diluent to form a tight network structure, thereby improving the friction resistance of the ink.

[0095] Combining Examples 1-3 and Comparative Example 2 and Table 1, it can be seen that the test data of Examples 1-3 are better than those of Comparative Example 2, indicating that the friction resistance of the ink is related to the type of resin selected. When the resin is an aliphatic epoxy resin, the ink can obtain better wear resistance. When other types of epoxy resins are selected, the curing time is extended, resulting in a loose structure, thereby reducing the friction resistance of the ink.

[0096] Combining Examples 1-3 and Comparative Example 3 and Table 1, it can be seen that the various test data of Examples 1-3 are better than those of Comparative Example 3, indicating that the polyethylene wax powder modified with polytetrafluoroethylene has good wear resistance and can be mixed into the ink system while ensuring a matte effect and improving the friction resistance of the ink.

[0097] Combining Examples 1-3 and Comparative Example 4 and Table 1, it can be seen that the various test data of Examples 1-3 are better than those of Comparative Example 4, indicating that when a free radical initiator is used, the shrinkage of the ink surface is not large, which affects the matte effect of the ink surface, and the initiator has a low initiation efficiency, resulting in a decrease in wear resistance.

[0098] Combining Examples 1-5 and Table 1, it can be seen that when the photoinitiator uses any one of iodonium salts, sulfonium salts and iron aromatics, inks with good matte effect and good wear resistance can be obtained; combining Examples 1-3, Example 6 and Comparative Example 5 and Table 1, it can be seen that when the example uses a mixture of talcum powder and ceramic powder as an inorganic filler, an ink with better matte effect and wear resistance can be obtained than when a single inorganic filler is used.

[0099] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A UV matte ink for mobile phone protective film, It is characterized in that It includes the following raw materials in parts by weight: 40-50 parts of modified epoxy acrylic resin, 40-50 parts of polyester resin, 20-30 parts of active diluent, 20-30 parts of photoinitiator, 3-5 parts of colorant, 3-10 parts of inorganic filler, and 5-10 parts of modified polyethylene wax powder.

2. A mobile phone protective film UV matte ink according to claim 1, Features: The modified epoxy acrylic resin is obtained by modification with hydroxyethyl methacrylate.

3. A mobile phone protective film UV matte ink according to claim 2, Features: The preparation method of the modified epoxy acrylic resin is as follows: (1) Mix epoxy resin and acrylic acid and heat to 70-80°C, slowly add dimethylaniline and azobisisobutyronitrile and heat to 80-110°C, keep warm for reaction, terminate the reaction when the acid value is lower than 6 mgKOH / g, cool naturally to obtain epoxy acrylic resin; (2) The epoxy acrylic resin obtained above is mixed evenly with hydroxyethyl methacrylate, triethylamine and dimethylaniline, and the mixture is heated to 60-80°C for reaction for 15-20 hours, precipitated with ether three times, and dried to obtain an epoxy resin modified with hydroxyethyl methacrylate.

4. The UV matte ink for mobile phone protective film according to claim 1, Features: The epoxy resin is an aliphatic epoxy resin.

5. The UV matte ink for mobile phone protective film according to claim 1, Features: The modified polyethylene wax powder is obtained by modifying polytetrafluoroethylene.

6. The UV matte ink for mobile phone protective film according to claim 1, Features: The photoinitiator is a cationic photoinitiator, which is one of iodonium salt, sulfonium salt and iron aromatic hydrocarbon.

7. The UV matte ink for mobile phone protective film according to claim 1, Features: The powder filler is a mixture of talcum powder and any one of quartz powder and ceramic powder; the particle size of the talcum powder is 2.5-2.7 μm, the particle size of the quartz powder is 1.3-1.6 μm, and the particle size of the ceramic powder is 4.5-5 μm.

8. A method for preparing a UV matte ink for a mobile phone protective film according to any one of claims 1 to 7, It is characterized in that The preparation method is as follows: (1) mixing and grinding the modified polyethylene wax powder and the inorganic filler to obtain a mixed inorganic filler; (2) Weighing modified epoxy acrylic resin and polyester resin and dissolving them in water, adding active diluent, photoinitiator, colorant and the mixed inorganic filler in step (1) in sequence, and ultrasonicating for 30 minutes to fully mix the components to obtain UV matte ink for mobile phone protective film.