A method for repairing positive electrode material of lithium ion battery and positive electrode material thereof
By chemically removing metal impurities in lithium-ion battery cathode materials and optimizing the roasting steps, the high cost and poor performance problems of the cathode material recycling process in the existing technology have been solved, and efficient and environmentally friendly cathode material repair has been achieved, improving the efficiency of the cathode material recovery process. Electrochemical performance and resource utilization.
Patent Information
- Application Number
- CN202310527373.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-05-08
AI Technical Summary
The existing lithium-ion battery cathode material recycling process has problems such as cumbersome acid-base wastewater treatment, irritating gas emissions, active material lattice changes, and lithium ion volatilization, resulting in high costs and poor performance.
Chemical methods are used to remove aluminum, magnetism and copper. Alkali solution and ions ranked before copper in the metal activity sequence are used to remove impurities. The steps of pole piece de-powdering, crushing, roasting and sieving are combined to strictly control the roasting temperature. and time to repair the cathode material.
It achieves a simple, economical and environmentally friendly cathode material repair process, improves the purity and electrochemical performance of the material, reduces production costs, and improves resource utilization.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure HDA0004244044890000011
Abstract
Description
Technical Field
[0001] The present invention relates to the field of waste recycling technology, H01M10 / 54, and in particular to a method for repairing a positive electrode material of a lithium ion battery and a positive electrode material thereof. Background Art
[0002] With the continued popularity of new energy vehicles, the demand for power batteries has increased significantly, leading to a surge in the price of raw materials for lithium-ion batteries; however, global lithium, cobalt, and nickel resources are mostly concentrated overseas and are monopolized by leading mining groups, which has greatly restricted my country's imports of raw materials. Especially since 2020, raw material companies have failed to implement their expansion plans as expected, resulting in a shortage of raw material imports and an even tighter supply. Among them, the price of lithium, known as "white oil", has doubled, causing the cost of positive electrode materials to rise rapidly; however, the cost of positive electrode materials in lithium batteries accounts for about 60%, and reducing the production cost of positive electrode materials is urgent.
[0003] The production process of lithium-ion batteries is relatively cumbersome and complicated. Each process affects whether the battery can be shipped out of the factory. Strengthening the management of defective and scrapped products in the actual production process and realizing resource reuse is an effective way to reduce production costs. In addition, lithium-ion batteries will gradually fail after about 5-7 years of use. The most obvious manifestation is the reduction in the capacity of the positive electrode material. During the long-term use of lithium-ion batteries, as lithium ions are constantly embedded and removed from the structure, the structure of the positive electrode material will change to a certain extent, resulting in lithium deficiency in the positive electrode material and reduced capacity. How to recycle and repair these defective batteries, produce scrapped batteries and a large number of waste batteries with positive electrode materials has become the most effective way to reduce the cost of positive electrode materials and batteries, and it also has both economic and environmental significance.
[0004] The methods currently used mainly include wet recycling and pyrometallurgical recycling. In wet recycling, the positive electrode material is mainly subjected to acid treatment and step-by-step precipitation, and the product is reprocessed into a positive electrode active material. For example, Chinese patent CN112811404A discloses a method for recycling waste lithium iron phosphate positive electrode powder. In this method, the recovered positive electrode material is mixed with a first inorganic acid and a metal complexing agent, and then mixed with a second inorganic acid and hydrogen peroxide for oxidation, and then a third inorganic acid is added for mixed dissolution, and finally an alkali is added to adjust the pH to obtain iron phosphate, and then processed to prepare lithium iron phosphate. Although the lithium iron phosphate prepared by this method has high purity, a large amount of acid-base wastewater is generated in the process, and the post-processing procedure is cumbersome and the processing cost is high. In addition, irritating gases are emitted during the process, which is not conducive to the health of workers. Pyrometallurgical recycling is to recover active substances by crushing and calcining to remove materials such as binders and conductive agents, but it is easy to change the lattice of the active material, volatilize lithium ions, increase carbon content, etc., which affects the performance of the positive electrode material and the battery. How to make up for the defects in the current methods and provide a positive electrode material repair method that can be used for defective batteries and waste batteries, which is simple in process, economical, environmentally friendly, and has excellent electrochemical properties of the repaired positive electrode material, is of great practical significance. Summary of the invention
[0005] In order to solve the above technical problems, the present invention first provides a method for repairing positive electrode materials of lithium-ion batteries, which includes the steps of removing aluminum, magnetism and copper from recycled materials.
[0006] Furthermore, the recycled materials come from defective batteries, scrapped batteries in production, and positive electrode plate materials of waste batteries; the main components include lithium iron phosphate, electrode additives, PVDF glue, carbon, etc., such as lithium iron phosphate positive electrode plates of carbon foil coated system.
[0007] Furthermore, the method uses chemical methods to remove aluminum, magnetism and copper from the recycled materials. Traditional flotation, magnetic separation and other technologies for removing metal impurities have many process requirements and require strict control of process conditions to separate metals of different densities, but the loss of active ingredients in the process cannot be avoided, and the process operation is complicated, the instrument cost is high, and the scope of use is small; while the present application uses chemical methods to remove metal impurities, which has stronger selectivity for metal impurities, higher impurity removal efficiency, high material purity, and simpler and more economical process.
[0008] Furthermore, alkaline solution is used to remove aluminum from the recycled materials. Specifically, the recycled materials are added to the alkaline solution for alkaline washing; the aluminum removal principle is:
[0009] Al+0H - →AlO 2 - .
[0010] Furthermore, the concentration of the alkali solution is 0.05-7 mol / L, and the alkali washing time is 10-250 min; preferably, the concentration of the alkali solution is 0.05-5 mol / L, and the alkali washing time is 10-120 min.
[0011] Furthermore, the concentration of the recycled material in the alkali solution is 10-50wt%, preferably 20-40wt%.
[0012] Furthermore, the alkaline washing process can be carried out with heating or at room temperature, depending on actual needs; preferably at room temperature.
[0013] Furthermore, in the aluminum removal of the recycled materials, the alkali solution is selected from any one or a combination of inorganic alkali and organic alkali.
[0014] Furthermore, the inorganic base includes but is not limited to at least one of lithium hydroxide, sodium hydroxide, potassium hydroxide, magnesium hydroxide, calcium hydroxide, sodium carbonate, potassium carbonate, and sodium amide.
[0015] Furthermore, the organic base includes but is not limited to at least one of alkylphenylammonium hydroxide, alkylammonium hydroxide, cycloalkylamine, sodium alkoxide, potassium alkoxide, alcoholamine, and alkyllithium.
[0016] In a preferred embodiment, the alkali solution is an inorganic base.
[0017] Furthermore, in the method, the demagnetization and copper removal of the recycled material can be performed simultaneously or sequentially; specifically, the recycled material is added to a solution of special ions for reaction, and the special ions are ions of metals that are ranked before copper in the metal activity sequence table. The principle is:
[0018] M a+ +Fe→Fe 2+ +M b+
[0019] M a+ +Cu→Cu 2+ +Mb + ;
[0020] where b <a。
[0021] Furthermore, the metal ions that precede copper in the metal activity sequence are selected from Fe 3+ Sn 4+ 、Al 3+ At least one of .
[0022] In the technical solution of the present application, the ions of the metal that ranks before copper in the metal activity sequence table are selected to oxidize iron and copper to remove them. Compared with the strong acid and hydrogen peroxide impurity removal in the traditional process, the impurity removal reaction of the present application is safer and non-irritating; Fe is selected 3+ Used in the process of demagnetization and copper removal, Fe 3+ It has stronger selectivity for iron and copper elements and higher impurity removal efficiency. Only adding this substance can realize the simultaneous execution of two processes, which reduces the types of ions in the treated filtrate and simplifies the post-processing operation flow of the solution. In addition, the ferrous ions generated after the reaction are components contained in the lithium iron phosphate material itself and will not reduce the purity of the material.
[0023] Preferably, the steps of removing magnetism and copper from the recycled material are carried out simultaneously, and the metal ions that are ranked before copper in the metal activity sequence are Fe 3+ .
[0024] Furthermore, the ion concentration of the metal before copper in the metal activity sequence is 0.05-20 mol / L, and the reaction time is 10-250 min; preferably, the ion concentration is 0.05-10 mol / L, and the reaction time is 10-180 min.
[0025] Furthermore, the concentration of the recycled material in the solution containing the special ions is 10-50wt%, preferably 20-40wt%.
[0026] Furthermore, the special ion solution includes but is not limited to any one or a combination of special ion halide solution, nitrate solution, sulfate solution, phosphate solution, and sulfide solution.
[0027] Preferably, the method for repairing the positive electrode material further comprises the steps of de-powdering, crushing and roasting the electrode pieces.
[0028] Preferably, the method for repairing the positive electrode material comprises the following steps in sequence:
[0029] S1, the electrode powder is removed;
[0030] S2, aluminum removal from recycled materials;
[0031] S3, demagnetization and copper removal of recycled materials;
[0032] S4, crushing;
[0033] S5, baking and degumming;
[0034] S6. Screening and demagnetization.
[0035] Furthermore, the electrode powder removal is specifically as follows: water is added to the graded filtration reactor, heating is turned on, and after reaching a certain temperature, the lithium iron phosphate positive electrode is put in, and after stirring, the primary filter is taken out, and the recycled materials of the secondary filter and the tertiary filter are collected.
[0036] Furthermore, the pole piece is a lithium iron phosphate positive pole piece of a carbon-coated foil system.
[0037] Preferably, the temperature is 60-90°C, more preferably 60-80°C.
[0038] Furthermore, the present application does not specify the stirring time and stirring speed, and the material on the positive electrode plate can be removed; in some embodiments, the stirring speed is 80-1500r / min, and the stirring time is 5-60min.
[0039] Furthermore, the specifications of the secondary filter screen and the tertiary filter screen are 10-30 mesh and 40-80 mesh respectively.
[0040] Furthermore, the S2 is specifically as follows: removing the grading filter, adding alkali solution to a certain concentration into the reactor of S1, then adding the recovered material of S1, stirring and alkali washing for a period of time, then washing, filtering and drying, and collecting the S2 material.
[0041] Furthermore, the S3 is specifically as follows: the material collected by S2 is put into a solution containing special ions of a certain concentration, stirred to react for a period of time, washed with water, filtered, and dried to obtain S3 material.
[0042] Furthermore, the solid content of the material collected in S2 in the solution is 10-50wt%.
[0043] Furthermore, after the water washing and filtration, the moisture content in the material of S3 must be kept below 1000ppm, further below 500ppm, and more preferably below 350ppm. When the moisture content is high, it will lead to uneven particle size distribution of the material in the subsequent pulverization process of S4, seriously affecting the efficiency and degree of subsequent degumming, and reducing the purity of the material.
[0044] Furthermore, step S4 is to crush the material S3, and the particle size requirements of the crushed material are: D50<1.5μm, Dmax<15μm. This application has no specific requirements for the crushing equipment, and at least one of the air flow mill, mechanical mill, and ball mill can be selected.
[0045] Furthermore, when the recycled materials of the present application come from the positive electrode plate materials of defective batteries or scrapped batteries in production, that is, when the positive electrode materials have not been used for charging and discharging, step S4 does not need to supplement lithium and can be directly crushed.
[0046] Furthermore, when the recycled material of the present application comes from the positive electrode plate material of waste batteries, that is, when the positive electrode material has been overcharged and discharged, step S4 needs to supplement lithium by mixing a certain amount of lithium salt and S3 material and then directly crushing them.
[0047] Furthermore, the amount of the lithium salt added is based on actual needs, and the lithium salt includes but is not limited to at least one of lithium oxalate, lithium acetate, lithium carbonate, lithium hydroxide monohydrate and lithium dihydrogen phosphate.
[0048] The roasting process in the present invention is mainly for degumming, but under high temperature roasting, the crystal form and crystallinity of the material may also change to a certain extent. The appropriate roasting temperature can not only achieve complete degumming, but also improve the crystallinity of the material, which is beneficial to the improvement of material structure and electrochemical performance, especially after lithium supplementation in S4, the effect of roasting on electrochemical performance is more obvious. When the roasting temperature is too low, the conductive glue cannot be completely removed and is not conducive to the migration and recombination of ions, and the purity of the material is low; when the temperature is too high, it will cause changes or decomposition of the crystal structure, which not only affects the embedding and migration of lithium ions, but also promotes the volatilization of lithium in the material, and the unevenness of the crystal particle size will increase; roasting too high or too long will lead to an increase in the carbon content in the material, which is not conducive to electrochemical performance. Therefore, it is necessary to strictly control the roasting temperature and time in this application, while achieving the purposes of complete degumming, avoiding lithium volatilization losses, and improving the electrochemical performance of materials.
[0049] Furthermore, in said S5, the calcination temperature is 300-800°C, and the calcination time is 2-10 hours. Preferably, the calcination temperature is 350-700°C, and the calcination time is 5-9 hours.
[0050] Furthermore, the present application has no strict regulations on the roasting furnace used for roasting, and any one of roller furnace, push plate furnace, rotary furnace, etc. can be selected. After roasting in the present application, if the fluorine content in the material is less than 500ppm, it can be considered that the glue is completely removed.
[0051] Furthermore, in the S5, an inert atmosphere is introduced to control the oxygen content to be below 30 ppm, more preferably below 10 ppm. In the present application, when the oxygen content is too high, the divalent iron in the material will be oxidized at high temperature, and the content of trivalent iron in the material will increase, which will lead to the failure of the electrode and its battery.
[0052] Furthermore, the inert atmosphere includes but is not limited to at least one of nitrogen, argon, helium, xenon, and carbon dioxide.
[0053] Furthermore, the S6 is to remove magnetism by screening through an ultrasonic vibrating screen and an electromagnetic iron remover.
[0054] Furthermore, the present application also provides a positive electrode material repaired by the method, namely, lithium iron phosphate.
[0055] Furthermore, the method is used for the recycling process of the positive electrode sheet materials of defective batteries, scrapped batteries in production, and waste batteries. Preferably, it is used for the recycling process of the positive electrode sheet materials of qualified batteries and scrapped batteries in production; the battery has not undergone a charge and discharge process; and lithium supplementation is not required in step S4.
[0056] Beneficial Effects
[0057] 1. The repair method of this application specifically uses a chemical method to remove metal impurities in the recycled material, the process conditions are milder and the cost is lower; alkali solution is used to remove aluminum, and Fe is specifically used. 3+ The strong oxidizing property of the cathode material is used to undergo disproportionation reaction and oxidation reaction to remove the iron and copper elements, thereby achieving better impurity removal effect and higher material purity. The electrochemical performance of the cathode material repaired by this method is more excellent.
[0058] 2. This application strictly controls the calcination temperature and calcination time in the calcination and degumming process, reconstructs the crystal form of the material and the insertion and migration channels of lithium ions, and simultaneously achieves the goals of complete degumming, avoiding lithium volatilization loss, and improving the electrochemical performance of the material;
[0059] 3. The method of the present application can be used for the recycling process of the positive electrode sheet materials of defective batteries, scrapped batteries in production, and waste batteries. In particular, for the positive electrode sheet materials of defective batteries and scrapped batteries in production that have not been charged or discharged, the loss of lithium ions can be completely avoided due to the special roasting conditions. No lithium replenishment operation is required during the roasting process, which greatly reduces the production cost.
[0060] 4. The positive electrode material repaired by the method of the present application has a uniform particle size distribution, excellent material purity and electrical properties, the first charge and discharge efficiency can reach 98.8%, the capacity is also significantly improved, and can be reused as a battery-sustaining positive electrode material, thereby improving resource utilization and greatly reducing the production cost of the battery.
[0061] Instruction Manual
[0062] Figure 1 : SEM image of the positive electrode material prepared by the repair method of Example 1;
[0063] Figure 2 : SEM image of the positive electrode material prepared by the repair method of Comparative Example 1;
[0064] Figure 3 : Comparison of the first charge and discharge curves of button cells prepared using the positive electrode materials of Example 1 and Comparative Example 1. DETAILED DESCRIPTION
[0065] Example
[0066] Example 1
[0067] This embodiment provides a method for repairing a positive electrode material of a lithium-ion battery, which comprises the following steps in sequence:
[0068] S1. Powder removal of electrode: add pure water to the graded filtration reactor, turn on the heating, put in the lithium iron phosphate positive electrode (carbon-coated foil system) after reaching 75°C, stir at 150r / min for 30min, take out the primary filter, and collect the recycled materials from the secondary filter (20 mesh) and the tertiary filter (50 mesh);
[0069] S2, aluminum removal from recycled materials: remove the grading filter, add lithium hydroxide to the reactor of S1 to prepare alkaline solution and make the concentration of the alkaline solution 1 mol / L, then add the recycled materials of S1 until the solid content of the recycled materials in the reactor solution is 30wt%, stir and alkaline wash for 60 minutes, then wash with water, filter press and dry, and collect S2 materials;
[0070] S3, Recycling materials for demagnetization and copper removal: Put the materials collected in S2 into a 2 mol / L ferric chloride solution to make the solid content of the materials in the solution 30wt%, stir and react for 90min, wash with water, filter press and dry to obtain S3 materials; the water content in S3 materials is less than 350ppm;
[0071] S4, crushing: crush the S3 material in a jet mill;
[0072] S5, roasting and degumming: the crushed material is placed in a rotary kiln and roasted at 495°C for 7.5 hours, wherein nitrogen is introduced into the rotary kiln to control the oxygen content in the rotary kiln to be below 10ppm;
[0073] S6. Screening and demagnetization: The roasted materials are screened and demagnetized through ultrasonic vibration screen and electromagnetic iron remover, and finally packaged.
[0074] Example 2
[0075] This embodiment provides a method for repairing a positive electrode material of a lithium-ion battery, which comprises the following steps in sequence:
[0076] S1. Powder removal of electrode: add pure water to the graded filtration reactor, turn on the heating, put in the lithium iron phosphate positive electrode (carbon-coated foil system) after reaching 75°C, stir at 100r / min for 60min, take out the primary filter, and collect the recycled materials from the secondary filter (20 mesh) and the tertiary filter (50 mesh);
[0077] S2, aluminum removal from recycled materials: remove the grading filter, add sodium hydroxide to the reactor of S1 to prepare alkaline solution and make the concentration of the alkaline solution 7 mol / L, then add the recycled materials of S1 until the solid content of the recycled materials in the reactor solution is 40wt%, stir and alkaline wash for 10 minutes, then wash with water, filter press and dry, and collect S2 materials;
[0078] S3, Recycling materials for demagnetization and copper removal: Put the materials collected in S2 into a 10 mol / L ferric chloride solution to make the solid content of the materials in the solution 40 wt%, stir and react for 20 min, wash with water, filter press and dry to obtain S3 materials; the water content in S3 materials is less than 500 ppm;
[0079] S4, crushing: crush the S3 material in a jet mill;
[0080] S5, roasting and degumming: the crushed material is placed in a rotary kiln and roasted at 700°C for 5 hours, wherein nitrogen is introduced into the rotary kiln to control the oxygen content in the rotary kiln below 30ppm;
[0081] S6. Screening and demagnetization: The roasted materials are screened and demagnetized through ultrasonic vibration screen and electromagnetic iron remover, and finally packaged.
[0082] Example 3
[0083] This embodiment provides a method for repairing a positive electrode material of a lithium-ion battery, which comprises the following steps in sequence:
[0084] S1. Powder removal of electrode: add pure water to the graded filtration reactor, turn on the heating, put in the lithium iron phosphate positive electrode (carbon-coated foil system) after reaching 80°C, stir at 1000r / min for 5min, take out the primary filter, and collect the recycled materials from the secondary filter (20 mesh) and the tertiary filter (50 mesh);
[0085] S2, aluminum removal from recycled materials: remove the grading filter, add lithium hydroxide to the reactor of S1 to prepare alkaline solution and make the concentration of the alkaline solution 0.1 mol / L, then add the recycled materials of S1 until the solid content of the recycled materials in the reactor solution is 20wt%, stir and alkaline wash for 120 minutes, then wash with water, filter press and dry, and collect S2 materials;
[0086] S3, Recycling materials for demagnetization and copper removal: Put the materials collected in S2 into a 0.2 mol / L ferric chloride solution to make the solid content of the materials in the solution 20wt%, stir and react for 180min, wash with water, filter press and dry to obtain S3 materials; the water content in S3 materials is less than 800ppm;
[0087] S4, crushing: crush the S3 material in a jet mill;
[0088] S5, roasting and degumming: the crushed material is placed in a rotary kiln and roasted at 380°C for 9 hours, wherein nitrogen is introduced into the rotary kiln to control the oxygen content in the rotary kiln below 30ppm;
[0089] S6. Screening and demagnetization: The roasted materials are screened and demagnetized through ultrasonic vibration screen and electromagnetic iron remover, and finally packaged.
[0090] Comparative Example 1
[0091] This embodiment provides a conventional repair method for lithium-ion battery positive electrode materials, specifically: (1) placing a lithium iron phosphate positive electrode sheet in a roller furnace and calcining it at 550° C. (nitrogen atmosphere, oxygen content less than 10 ppm) for 5 hours;
[0092] (2) placing the calcined electrode sheet in (1) in a mechanical pulverizer for coarse crushing;
[0093] (3) The coarse crushed material in (2) is placed on a drum screen for screening, and the positive electrode material is finally selected.
[0094] Comparative Example 2
[0095] The method is basically the same as Example 1, except that: S5 is as follows: the crushed material is placed in a rotary kiln and roasted at 750°C for 9 hours, wherein nitrogen is introduced into the rotary kiln to control the oxygen content in the rotary kiln to be below 30 ppm.
[0096] Comparative Example 3
[0097] The method is basically the same as Example 1, except that in S5, the oxygen content in the rotary kiln is controlled at about 80 ppm.
[0098] Comparative Example 4
[0099] The method is basically the same as Example 1, except that the water content in the S3 material is 1000 ppm.
[0100] Comparative Example 5
[0101] The method is basically the same as Example 1, except that in S3, the solid content of the material in the solution is 60wt%.
[0102] Comparative Example 6
[0103] The method is basically the same as that in Example 1, except that in S3, the reaction time is 5 min.
[0104] Performance testing method: Analyze and characterize the positive electrode materials obtained by the repair methods of the above embodiments and comparative examples, including the content of each element of the active substance lithium iron phosphate, the content of other impurity metal elements, the particle size distribution of the material, etc.; and evaluate the electrochemical performance of the button batteries prepared therefrom; and judge the advantages and disadvantages of the methods and processes.
[0105] Performance test results:
[0106] The test results are shown in Table 1.
[0107] Table 1
[0108]
[0109]
[0110] The above results can be analyzed to conclude that the lithium iron phosphate positive electrode material prepared by the repair method of the present invention has a more uniform particle size distribution (smaller D100), low content of impurities and magnetic foreign matter, a higher capacity of 154.4 mAh / g, a stable voltage platform, a more delayed voltage drop (near 135 mAh / g), and excellent comprehensive electrochemical performance.
Claims
1. A method for repairing a positive electrode material of a lithium ion battery, characterized in that: The method comprises the steps of removing aluminum, removing magnetism and removing copper from the recycled material; in the method, the aluminum, magnetism and copper removal from the recycled material are all carried out by chemical methods; The demagnetization and decopperization of the recycled materials can be performed simultaneously or sequentially; specifically, the recycled materials are added to a solution of special ions for reaction, wherein the special ions are ions of metals that are ranked before copper in the metal activity sequence table; The steps of removing magnetism and copper from the recycled material are carried out simultaneously. The metal ion that is ranked before copper in the metal activity sequence is Fe 3+ ; The ion concentration of the metal before copper in the metal activity sequence is 0.05-20 mol / L, and the reaction time is 10-250 min; The method for repairing the positive electrode material comprises the following steps in sequence: S1, the electrode powder is removed; S2, aluminum removal from recycled materials; S3, demagnetization and copper removal of recycled materials; S4, crushing; S5, baking and degumming; S6, screening and demagnetization; The solid content of the material collected in S2 in the solution is 10-50wt%; The S3 is specifically as follows: the material collected in S2 is put into a solution containing special ions of a certain concentration, stirred for a period of time, washed with water, filtered, and dried to obtain the S3 material; After washing and filtration, the moisture content of S3 material must be kept below 1000ppm; The calcination temperature in S5 is 300-800°C and the calcination time is 2-10h Inert atmosphere is introduced into S5 to control the oxygen content to be below 30 ppm.
2. The repair method according to claim 1, characterized in that: The aluminum removal from the recycled materials is carried out using alkaline solution.
3. The positive electrode material prepared by the repair method according to claim 2.