Preparation method of p-type Bi2Te3-based thermoelectric material

Through high-energy ball milling and SPS sintering processes, the Cu element content is adjusted to improve the conductivity of p-type Bi2Te3-based thermoelectric materials, solving the problem of insufficient conductivity of existing materials and achieving efficient thermoelectric material preparation.

CN116693292BActive Publication Date: 2024-10-01XI AN JIAOTONG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310661743.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-06
Publication Date
2024-10-01
Estimated Expiration
2043-06-06

AI Technical Summary

Technical Problem

Existing commercial p-type Bi2Te3-based thermoelectric materials have insufficient electrical conductivity and are difficult to meet certain applications requiring high electrical conductivity.

Method used

High-energy ball milling method combined with SPS sintering process was used to increase the electrical conductivity by adjusting the content of Cu element (the value of x ranges from 0 to 0.15), and prepared p-type Bi2Te3-based thermoelectric materials with high electrical conductivity.

Benefits of technology

Significantly improves the conductivity of the material, which is more than 2 times that of commercial materials. It is suitable for high conductivity applications in the medium and low temperature range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116693292B_ABST
    Figure CN116693292B_ABST
Patent Text Reader

Abstract

Disclosed is a method for preparing a p-type Bi2Te3-based thermoelectric material and a thermoelectric material. The method comprises the following steps: using Bi, Cu, Sb, and Te as raw materials, and preparing the thermoelectric material according to the chemical formula Bi 0.5 Cu 2x Sb 1.5 Te 3+x After weighing, mix and put into a ball mill, wherein the value range of x is 0 to 0.15; the raw materials in the ball mill are milled by a ball mill to obtain powder; the powder after ball milling is sintered by SPS sintering method under vacuum pressure conditions to form p-type Bi2Te3-based thermoelectric materials. This method significantly improves the electrical conductivity, and micro-nano powders of different sizes can be obtained by combining high-energy ball milling with SPS sintering process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure belongs to the technical field of thermoelectric materials, and in particular relates to a method for preparing a p-type Bi2Te3-based thermoelectric material. Background Art

[0002] Thermoelectric material is a functional material that can realize the conversion of heat energy and electric energy. Thermoelectric conversion technology is based on the Seebeck effect. It can realize the mutual conversion of heat energy and electric energy by driving the migration of carriers by temperature difference to form thermoelectric potential. Thermoelectric power generation devices made of thermoelectric materials can use industrial and commercial waste heat, geothermal heat, human body temperature, etc. as heat sources for thermoelectric conversion, and have the advantages of small size, high stability, long life, green environmental protection, and maintenance-free. Energy and environmental problems in the world today are becoming increasingly serious. Making full use of energy resources and improving energy utilization efficiency have become the current research on thermoelectricity. Thermoelectric conversion technology can realize the conversion of low-grade heat sources and waste heat into electrical energy, and has broad application prospects in the field of energy resource utilization.

[0003] Thermoelectric figure of merit (dimensionless ZT value) is an indicator to measure the thermoelectric conversion efficiency of thermoelectric materials. Thermoelectric materials with high thermoelectric conversion efficiency often have larger thermoelectric figure of merit. ZT can be expressed as:

[0004]

[0005] Where S is the Seebeck coefficient, which is the electromotive force generated by the unit gradient temperature of the material. Its magnitude depends on the type of carriers and the temperature difference between the two ends of the material. σ is the electrical conductivity, which is related to the carrier concentration and carrier mobility. κ is the thermal conductivity, which is composed of electronic thermal conductivity and lattice thermal conductivity. Thermoelectric materials with higher thermoelectric figures of merit often have higher Seebeck coefficients, larger electrical conductivity, and lower thermal conductivity, but the relationship between these three is mutually coupled and mutually influential, and comprehensive regulation is more difficult. Bi2Te3-based thermoelectric materials are a type of thermoelectric material suitable for low temperatures (room temperature-300°C), and this type of material has been commercialized. The electrical conductivity of commercial p-type Bi2Te3 materials at room temperature is generally 10 5 S / m. In some applications with higher conductivity requirements, the conductivity of commercial p-type Bi2Te3 materials is slightly insufficient. Therefore, improving the conductivity of p-type Bi2Te3-based thermoelectric materials for these usage scenarios has become one of the problems that need to be solved.

[0006] The above information disclosed in this Background section is only for enhancement of understanding of the background of the invention and therefore it may contain information that does not form the prior art that is already known to a person of ordinary skill in the art. Summary of the invention

[0007] In view of the deficiencies in the prior art, the present invention aims to provide a method for preparing a p-type Bi2Te3-based thermoelectric material with high electrical conductivity.

[0008] To achieve the above objectives, the present disclosure provides the following technical solutions:

[0009] A method for preparing a p-type Bi2Te3-based thermoelectric material comprises the following steps:

[0010] Bi, Cu, Sb, Te are used as raw materials, according to the thermoelectric material chemical formula Bi 0.5 Cu 2x Sb 1.5 Te 3+x After weighing, mix and put into a ball mill, wherein the value range of x is 0 to 0.15;

[0011] The ball mill grinds the raw materials in the ball mill jar to obtain powder;

[0012] The powder after ball milling is sintered by SPS sintering method under vacuum pressure conditions to form p-type Bi2Te3-based thermoelectric materials.

[0013] In the method, the powder after ball milling is subjected to SPS sintering in a vacuum glove box under the protection of argon atmosphere.

[0014] In the method, the ball mill and the grinding balls are made of stainless steel, the grinding aid is anhydrous ethanol, and the ball mill after mixing is vacuum-sealed.

[0015] In the method, the ball mill is a planetary ball mill.

[0016] In the method described, the total rotation speed of the planetary ball mill is 500 rpm, the rotation speed of the self-rotating disk is 1000 rpm, and the rotation speed of the orbiting disk is 500 rpm.

[0017] In the method, the ball mill performs intermittent ball milling; the intermittent ball milling is performed by pausing for 15 minutes after each ball milling for 40 minutes, and the total ball milling time is 8 hours.

[0018] In the method, the ball-milled powder is dried in a vacuum oven with a vacuum degree of ≤0.1 Pa, a drying temperature of 70-100° C., and a drying time of ≥18 h.

[0019] In the method described, the temperature of the vacuum oven is increased by gradient heating; the gradient heating is to increase the temperature to 70°C in 30 minutes, keep the temperature for 5 hours, then increase the temperature to 100°C in 2 hours, and continue to keep the temperature.

[0020] In the method, the dried powder material is sieved using an ultrasonic vibration screen; the mesh number of the vibration screen is ≥450 meshes.

[0021] The p-type Bi2Te3-based thermoelectric material is prepared according to the described method.

[0022] Compared with the prior art, the present invention has the following beneficial effects: thermoelectric materials are prepared by high-energy ball milling combined with SPS sintering. High-energy ball milling can greatly reduce the powder preparation cycle, and vacuum sealing can effectively prevent the volatilization of raw materials after the ball milling process. SPS sintering speed is fast, and the density of the sintered bulk material is good, which greatly improves the efficiency of thermoelectric material preparation. The method of the present invention can quickly and efficiently prepare Bi 0.5 Cu 2x Sb 1.5 Te 3+x , where x is determined by the proportion of Cu element in the total mass, and typical values ​​can be 0.032, 0.065, and 0.13. The more suitable value range of x is 0-0.15. If x is too small, the effect of performance regulation is limited. As the value of x increases, the regulation effect will gradually approach saturation. If x exceeds 0.15, the change in performance parameters is very small. The addition of additional Cu elements can significantly improve the conductivity. Micro-nano powders of different sizes can be obtained by high-energy ball milling combined with SPS sintering process. When x = 0.065, the sample Bi 0.5 Cu 0.13 Sb 1.5 Te 3.065 The conductivity is as high as 2.7×10 at 308K. 5 S / m is the conductivity of the currently commercially available p-type Bi2Te3-based thermoelectric material (in 10 5 S / m) more than twice. 0.5 Cu 2x Sb 1.5 Te 3+x Thermoelectric materials have good application prospects in situations where high electrical conductivity is required in the medium and low temperature range. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is the p-type Bi mentioned in the embodiment 0.5 Cu 0.13 Sb 1.5 Te 3.065 Thermoelectric material preparation process flow chart;

[0024] Figure 2 is the p-type Bi mentioned in the embodiment 0.5 Cu 0.13 Sb 1.5 Te 3.065 SEM images of thermoelectric materials;

[0025] Figure 3 is the p-type Bi mentioned in the embodiment 0.5 Cu 0.13 Sb1.5 Te 3.065 Graph of the relationship between the Seebeck coefficient of thermoelectric materials and temperature;

[0026] Figure 4 is the p-type Bi mentioned in the embodiment 0.5 Cu 0.13 Sb 1.5 Te 3.065 A graph showing the relationship between the conductivity of thermoelectric materials and temperature;

[0027] Figure 5 is the p-type Bi mentioned in the embodiment 0.5 Cu 0.13 Sb 1.5 Te 3.065 A graph of the power factor of a thermoelectric material versus temperature;

[0028] Figure 6 is the p-type Bi mentioned in the embodiment 0.5 Cu 0.13 Sb 1.5 Te 3.065 Graph of thermal conductivity of thermoelectric materials versus temperature;

[0029] Figure 7 is the p-type Bi mentioned in the embodiment 0.5 Cu 0.13 Sb 1.5 Te 3.065 A graph showing the relationship between the ZT value of thermoelectric materials and temperature. DETAILED DESCRIPTION

[0030] The following will refer to the attached Figure 1 To Attachment Figure 7 Specific embodiments of the present disclosure are described in detail. Although specific embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments described herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.

[0031] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the difference in the functions of the components as the criterion for distinction. As mentioned throughout the specification and claims, "including" or "comprising" is an open term, so it should be interpreted as "including but not limited to". The subsequent description of the specification is a preferred embodiment of the present invention, but the description is based on the general principles of the specification and is not used to limit the scope of the present invention. The scope of protection of the present disclosure shall be determined by the attached claims.

[0032] To facilitate understanding of the embodiments of the present disclosure, further explanation will be given below using specific embodiments as examples in conjunction with the accompanying drawings, and each of the accompanying drawings does not constitute a limitation on the embodiments of the present disclosure.

[0033] like Figures 1 to 7 As shown, a method for preparing a p-type Bi2Te3-based thermoelectric material comprises the following steps:

[0034] Bi, Cu, Sb, Te are used as raw materials, according to the thermoelectric material chemical formula Bi 0.5 Cu 2x Sb 1.5 Te 3+x After weighing, mix and put into a ball mill, where x is determined according to the proportion of Cu element in the total mass, and the typical value can be 0.032, 0.065, 0.13. The more suitable value range of x is 0-0.15. If x is too small, the effect of performance regulation is limited. As the value of x increases, the regulation effect will gradually approach saturation. If x exceeds 0.15, the change in performance parameters is very small;

[0035] The ball mill grinds the raw materials in the ball mill jar to obtain powder;

[0036] The powder after ball milling is sintered by SPS sintering method under vacuum pressure conditions to form p-type Bi2Te3-based thermoelectric materials.

[0037] In a preferred embodiment of the method, the powder after ball milling is subjected to SPS sintering in a vacuum glove box under the protection of argon atmosphere.

[0038] In a preferred embodiment of the method, the ball mill and the grinding balls are made of stainless steel, and the grinding aid is anhydrous ethanol; and the ball mill after mixing is vacuum-sealed.

[0039] In a preferred embodiment of the method, the ball mill is a planetary ball mill.

[0040] In a preferred embodiment of the method, the total rotation speed of the planetary ball mill is 500 rpm, the rotation speed of the self-rotating disk is 1000 rpm, and the rotation speed of the orbiting disk is 500 rpm.

[0041] In a preferred embodiment of the method, the ball mill performs intermittent ball milling; the intermittent ball milling is performed by pausing for 15 minutes after each 40 minutes of ball milling, and the total ball milling time is 8 hours.

[0042] In a preferred embodiment of the method, the ball-milled powder is dried in a vacuum oven with a vacuum degree of ≤0.1 Pa, a drying temperature of 70-100° C., and a drying time of ≥18 h.

[0043] In a preferred embodiment of the method, the temperature of the vacuum oven is increased by gradient heating; the gradient heating is to increase the temperature to 70°C in 30 minutes, keep the temperature for 5 hours, then increase the temperature to 100°C in 2 hours, and continue to keep the temperature.

[0044] In a preferred embodiment of the method, the dried powder material is sieved using an ultrasonic vibration screen; the mesh number of the vibration screen is ≥450 meshes.

[0045] In a preferred embodiment of the method, the initial SPS sintering temperature is room temperature, the sintering temperature is 350°C to 450°C, the pressure is 50 to 65 MPa, and the holding time is 10 min.

[0046] In one embodiment, the chemical formula of the prepared material is Bi 0.5 Cu 2x Sb 1.5 Te 3+x , where x is determined according to the proportion of Cu element in the total mass, and typical values ​​can be 0.032, 0.065, and 0.13. The more suitable value range of x is 0 to 0.15. If x is too small, the effect of performance regulation is limited. As the value of x increases, the regulation effect will gradually approach saturation. If x exceeds 0.15, the change in performance parameters is very small. The preparation method of the p-type Bi2Te3-based thermoelectric material comprises:

[0047] (1) Component ratio: weigh Bi, Cu, Sb, and Te single-element raw materials and put them into the ball mill;

[0048] (2) Powder preparation: a high-energy ball milling method is used to prepare the powder, and the ball mill is placed on a planetary ball mill for 8 hours;

[0049] (3) Powder processing: after ball milling, the powder is sieved and vacuum dried;

[0050] (4) Block sintering: The dried powder is placed in an SPS sintering furnace for sintering.

[0051] In the step of proportioning the ingredients, the raw materials were weighed in a glove box protected by an argon atmosphere. 0.5 Cu 2x Sb 1.5 Te 3+x , that is, according to the mass ratio Bi:Cu:Sb:Te=104.49:127.09x:182.55:(382.8+127.6x), the single-substance raw materials are weighed in the glove box and put into the stainless steel ball mill, which is filled with three sizes of grinding balls: Φ20mm grinding balls 80.23g, Φ15mm grinding balls 78.95g, Φ8mm grinding balls 60.86g, Φ6mm grinding balls 80.8g, Φ4mm grinding balls 30.68g, the total mass of the grinding balls is 331.52g, the mass of the powder is controlled at 10g~20g, and the ball-to-material ratio is below 1:30. Pour anhydrous ethanol into the ball mill, the amount of anhydrous ethanol slightly covers all the fillers, but ensure that the liquid level of anhydrous ethanol does not exceed 1 / 3 of the volume of the ball mill. After all the materials are filled, the ball mill is placed in the transition chamber of the glove box, vacuumed and sealed, and then taken out for ball milling.

[0052] In the process of powder preparation, the ball milling treatment method selected is intermittent ball milling. The intermittent ball milling is to pause for 15 minutes after each ball milling for 40 minutes, and the total ball milling time is 8 hours. Intermittent ball milling is to prevent the powder from sticking to the wall and affecting the ball milling efficiency on the one hand, and to protect the motor on the other hand. The working parameters of the ball mill are set as follows: the total speed of the ball mill is 500rpm, the speed of the self-rotating disk is 1000rpm, and the speed of the revolving disk is 500rpm. The powder after ball milling needs to be vacuum dried. The vacuum degree of the drying oven is ≤0.1Pa. It is first heated to 70℃ after 30min, kept warm for 5h, and then heated to 100℃ for 2h and continued to keep warm. The total insulation time is more than 18h. The purpose of using the gradient heating method is to volatilize the ethanol liquid under low-temperature vacuum conditions, and then dry the remaining powder completely at high temperature. The dried powder material is sieved using an ultrasonic vibrating screen, and the mesh number of the vibrating screen is ≥450 mesh. Powders of different particle sizes are separated by sieving, and impurities with larger particle sizes can be screened out.

[0053] During the block sintering process, SPS sintering is selected. In an optional embodiment, the SPS sintering parameters include: the initial temperature is room temperature, the sintering temperature is 350℃~450℃; the pressure is 50~65MPa; the holding time is 10min. The sintering process adopts gradient heating and full pressure holding; the gradient heating and full pressure holding are 10min from room temperature to 250℃, then 5min to 450℃, holding for more than 10min, and then cooling with the furnace; the pressure is kept loaded during the whole sintering process.

[0054] In the present invention, high-energy ball milling and SPS sintering process are used to better avoid the shortcomings of traditional synthesis methods. Among them, high-energy ball milling does not require high-temperature reaction conditions, thereby avoiding the vaporization of reaction raw materials and causing excessive vapor pressure, which brings potential safety hazards. The traditional melting method requires a long insulation time and annealing time, and the general cycle requires 10 days or more. Compared with the melting method, high-energy ball milling combined with SPS sintering process can greatly reduce the preparation cycle of the material and improve the preparation efficiency. In addition, the melting method can produce nanoscale powders, which can enhance the scattering of short-wavelength phonons, while high-energy ball milling combined with SPS sintering process can prepare micro-nano full-scale powders, which have a good scattering effect on short-wavelength and long-wavelength phonons, and can further reduce the thermal conductivity of the material.

[0055] Preferably, the raw materials are weighed in a glove box protected by an argon atmosphere.

[0056] Preferably, the ball mill and the grinding balls are made of stainless steel, and the grinding aid is anhydrous ethanol.

[0057] Preferably, the ball mill jar after mixing needs to be vacuum-sealed before ball milling.

[0058] Preferably, the ball milling treatment method is intermittent ball milling. The intermittent ball milling is performed by pausing for 15 minutes after each 40 minutes of ball milling, and the total ball milling time is 8 hours. Intermittent ball milling is used to prevent the powder from sticking to the wall and affecting the ball milling efficiency, and to protect the motor.

[0059] Preferably, the total speed of the ball mill is 500 rpm, the speed of the self-rotating disk is 1000 rpm, and the speed of the revolving disk is 500 rpm.

[0060] Preferably, the powder after ball milling needs to be vacuum dried. The vacuum degree of the drying oven is ≤0.1Pa. The temperature is first raised to 70°C for 30 minutes, kept warm for 5 hours, and then raised to 100°C for 2 hours and kept warm. The total insulation time is more than 18 hours. The purpose of using a gradient heating method is to volatilize the ethanol liquid under low-temperature vacuum conditions, and then dry the remaining powder completely at high temperature.

[0061] Preferably, the dried powder material is sieved using an ultrasonic vibrating screen with a mesh size of ≥450. Sieving can separate powders of different particle sizes and can also screen out impurities with larger particle sizes.

[0062] On the other hand, the present invention also provides a p-type Bi2Te3-based thermoelectric material prepared according to the above-mentioned preparation method.

[0063] On the other hand, the present invention also provides a p-type Bi2Te3-based thermoelectric material dense block, using the above-mentioned p-type Bi2Te3-based thermoelectric material as a raw material, and obtaining the p-type Bi2Te3-based thermoelectric material dense block through SPS sintering; SPS sintering parameters are: initial temperature is room temperature, sintering temperature is 350℃~450℃; pressure is 50~65MPa; insulation time is 10min. The sintering process adopts gradient heating and full pressure maintenance; the gradient heating and full pressure maintenance are 10min from room temperature to 250℃, then 5min to 450℃, insulation for more than 10min, and then cooling with the furnace; the pressure is kept on during the whole sintering process.

[0064] Example

[0065] Take x value as 0.065 to prepare p-type Bi 0.5 Cu 0.13 Sb 1.5 Te 3.065 Thermoelectric material: 2.6123 g of Bi single substance raw material, 0.2065 g of Cu single substance raw material, 4.5638 g of Sb single substance raw material, and 9.7774 g of Te single substance raw material were weighed in proportion in an argon atmosphere glove box and filled into a stainless steel ball mill.

[0066] The stainless steel ball mill is evacuated and sealed in the transition chamber, and then taken out for high-energy ball milling. In this embodiment, the speed of the revolution plate of the ball mill is 1000rpm, the speed of the rotation plate is 500rpm, and the intermittent ball milling method is adopted. After each 40min of ball milling, it pauses for 15min, and the total ball milling time is 30h. After the ball milling is completed, the powder is taken out and placed in a vacuum drying oven for drying. The vacuum degree of the drying oven is ≤0.1Pa. It is first heated to 70℃ for 30min, kept warm for 5h, and then heated to 100℃ for 2h, and continued to be kept warm for 16h. After the dried powder is taken out, it is sieved through a 450-mesh sieve, and then an appropriate amount of powder is weighed and pressed into a Φ20×3mm block material.

[0067] The pressed material is placed in the SPS sintering furnace and sintered under vacuum. The sintering temperature is 450℃, and the pressure applied during the sintering process is 50MPa. The sintering process adopts a gradient heating and full pressure maintenance method. It first heats from room temperature to 250℃ in 10 minutes, then heats to 450℃ in 5 minutes, keeps the temperature for more than 10 minutes, and then cools with the furnace; the pressure is maintained at 50Mpa during the whole sintering process.

[0068] The Seebeck coefficient and electrical conductivity were measured by the ZEM-3 thermoelectric performance analysis system, and the thermal conductivity was further calculated by the LFA-467 laser thermal conductivity meter. Finally, the prepared p-type Bi 0.5 Cu 0.13 Sb 1.5 Te 3.065The power factor and ZT value of thermoelectric materials. Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 As shown, at T = 308K, Bi 0.5 Cu 0.13 Sb 1.5 Te 3.06 The Seebeck coefficient of the thermoelectric block is 0.00011 V / K and the electrical conductivity is 2.7×10 5 S / m, power factor is 35W / m·K 2 , thermal conductivity is 1.9W / m·K, and ZT value is 0.68.

[0069] The basic principles of the present disclosure are described above in conjunction with specific embodiments. However, it should be noted that the advantages, strengths, effects, etc. mentioned in the present disclosure are only examples and not limitations, and it cannot be considered that these advantages, strengths, effects, etc. are required by each embodiment of the present disclosure. In addition, the specific details disclosed above are only for the purpose of illustration and ease of understanding, rather than limitation, and the above details do not limit the present application to the use of the above specific details to be implemented.

Claims

1. A method for preparing a p-type Bi2Te3-based thermoelectric material, characterized in that: It includes the following steps: Bi, Cu, Sb, Te are used as raw materials, according to the thermoelectric material chemical formula Bi 0.5 Cu 2x Sb 1.5 Te 3+x After weighing, mix and put into a ball mill, where the value of x ranges from 0.032 to 0.15; The ball mill grinds the raw materials in the ball mill jar to obtain powder; The powder after ball milling is sintered under vacuum pressure conditions using the SPS sintering method to form p-type Bi2Te3-based thermoelectric materials. The ball mill and the grinding balls are made of stainless steel, and the grinding aid is anhydrous ethanol. The ball mill after mixing is vacuum-sealed, and the powder after ball milling is dried in a vacuum drying oven with a vacuum degree of ≤0.1Pa, a drying temperature of 70-100°C, and a drying time of ≥18h. The vacuum drying oven is heated using a gradient heating method, which is to heat up to 70°C in 30min, keep warm for 5h, and then heat up to 100°C for 2h, and continue to keep warm. The sintering process uses a gradient heating method with full pressure maintenance. The gradient heating method and the full pressure maintenance method are to heat up from room temperature to 250°C in 10min, then heat up to 450°C in 5min, keep warm for more than 10min, and then cool with the furnace. The pressure is kept on during the entire sintering process.

2. The method according to claim 1, characterized in that The ball mill is a planetary ball mill.

3. The method according to claim 2, characterized in that The total rotation speed of the planetary ball mill is 500 rpm, the rotation speed of the self-rotating disk is 1000 rpm, and the rotation speed of the orbiting disk is 500 rpm.

4. The method according to claim 1, characterized in that The ball mill performs intermittent ball milling; the intermittent ball milling is performed by pausing for 15 minutes after each 40 minutes of ball milling, and the total ball milling time is 8 hours.

5. The method according to claim 1, characterized in that: The dried powder material is sieved using an ultrasonic vibration screen; the mesh number of the vibration screen is ≥450 meshes.

6. A p-type Bi2Te3-based thermoelectric material, characterized in that: It is prepared according to the method according to any one of claims 1 to 5.