A fluorinated graphene / metal oxide nanoparticle / organic amine composite coating and its preparation method and application

By introducing metal oxide nanoparticles and organic amines into fluorinated graphene, and using ultrasonic solvothermal method and aminoation treatment, the composite coating of fluorinated graphene/metal oxide nanoparticles/organic amines was constructed, and the graphene fluorinated graphene was solved. The problem of unstable adsorption of olefins and metal substrates significantly improves the lubricating and corrosion resistance of the coating, and is suitable for mechanical equipment protection in complex marine environments.

CN116694117BActive Publication Date: 2024-12-06LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310635913.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-01
Publication Date
2024-12-06
Estimated Expiration
2043-06-01

AI Technical Summary

Technical Problem

Fluorinated graphene is difficult to stably adsorb with the metal substrate surface when constructing protective coatings, resulting in unstable protective performance. The two-dimensional nanomaterial coating exhibits wear and corrosion risks under the coupling of friction and corrosion in complex marine environments. .

Method used

By introducing metal oxide nanoparticles and organic amines into graphene fluorinated, ultrasonic solvothermal method and aminoation treatment method are used to construct a composite coating of fluorinated graphene/metal oxide nanoparticles/organic amines to enhance its combination with metals Covalent bonding and wear resistance of the substrate.

Benefits of technology

The stability and corrosion resistance of the fluorinated graphene coating have been improved, the lubrication life and protection effect have been significantly improved, and the service life of the equipment has been extended in the marine environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116694117B_ABST
    Figure CN116694117B_ABST
Patent Text Reader

Abstract

The present invention provides a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating and a preparation method and application thereof, belonging to the technical field of composite materials. The present invention mixes a fluorinated graphene nanosheet (FG) alcohol dispersion and a metal oxide nanoparticle alcohol dispersion, performs a solvothermal reaction under ultrasonic conditions, and obtains a fluorinated graphene / metal oxide composite nanomaterial; the fluorinated graphene / metal oxide composite nanomaterial, a first organic amine and an alcohol solvent are mixed to obtain a film-forming liquid; a metal substrate is mixed with a second organic amine liquid, and an amination treatment is performed to obtain an amination-treated substrate; the film-forming liquid is made to form a film on the surface of the amination-treated substrate to obtain a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating. The present invention can construct a stable fluorinated graphene-based composite coating, and the obtained composite coating has excellent lubrication and corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite coatings, and in particular to a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating and a preparation method and application thereof. Background Art

[0002] For mechanical equipment, the main reason for its performance failure is friction and the resulting wear of parts. The characteristics of the marine environment, such as humidity, heat and high salt content, mean that mechanical equipment not only faces the risk of lubrication failure, but also faces the risk of equipment failure caused by chemical corrosion, electrochemical corrosion and biological corrosion, as well as the risk of increased material surface erosion behavior caused by friction-corrosion coupling under certain working conditions. Therefore, the design and development of integrated protective coating materials for friction and corrosion has become an important breakthrough in solving the problems of equipment lubrication and corrosion in complex marine environments.

[0003] Research has shown that due to the unique lamellar crystal structure with high specific surface area, the coating constructed by two-dimensional nanomaterials can hinder the penetration of external media such as gas, steam and liquid, and achieve corrosion protection for the base material through physical barriers. In addition, due to its unique layered crystal structure, two-dimensional nanomaterials have both low slip shear strength given by weak interlayer van der Waals forces and high in-plane mechanical strength given by in-plane covalent bonding, showing excellent structural lubrication and high bearing capacity, which makes two-dimensional nanomaterials show great application potential in the field of constructing integrated friction and corrosion protection nanocomposite coatings.

[0004] Fluorinated graphene (FG) is an important member of the two-dimensional material family. It is made by introducing the most electronegative F element into the graphene skeleton. On the basis of retaining the excellent mechanical properties, anti-permeability and chemical stability of the graphene carbon skeleton, the CF bond formed by the introduced fluorine element gives FG super hydrophobicity and insulation properties. On the basis of improving the corrosion resistance of FG against corrosive media, it effectively avoids the electrochemical corrosion problem of graphene materials, thus showing a stronger anti-corrosion potential. However, the high chemical stability and low surface energy characteristics of the CF bond make the binding performance of FG with the substrate even weaker than that of graphene, and it is difficult to physically / chemically adsorb on the metal substrate surface and build a stable protective coating like graphene oxide (GO). Summary of the invention

[0005] In view of this, the object of the present invention is to provide a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating and a preparation method and application thereof. The method provided by the present invention can construct a stable fluorinated graphene-based composite coating, and the obtained fluorinated graphene / metal oxide nanoparticle / organic amine composite coating has excellent lubricity and corrosion resistance.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating, comprising the following steps:

[0008] The fluorinated graphene nanosheet alcohol dispersion and the metal oxide nanoparticle alcohol dispersion are mixed, and a solvothermal reaction is carried out under ultrasonic conditions to obtain a fluorinated graphene / metal oxide composite nanomaterial;

[0009] Mixing the fluorinated graphene / metal oxide composite nanomaterial, a first organic amine and an alcohol solvent to obtain a film-forming solution;

[0010] The metal substrate is mixed with a second organic amine liquid and subjected to an amination treatment to obtain an amination-treated substrate;

[0011] The film-forming liquid is made to form a film on the surface of the heated amination-treated substrate to obtain a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating.

[0012] Preferably, the carbon-fluorine atomic ratio of the fluorinated graphene nanosheets is 1.05-1.8, and the average sheet diameter is 5-40 μm.

[0013] Preferably, the metal oxide is MoO 3 、MgO、CeO 2 、ZrO 2 , CuO and Y 2 O 3 One or more of the following;

[0014] The particle size of the metal oxide nanoparticles is 10 to 80 nm.

[0015] Preferably, the mass ratio of the metal oxide nanoparticles to the fluorinated graphene nanosheets is 1:4-20.

[0016] Preferably, the temperature of the solvent thermal reaction is 80 to 160° C., and the time is 0.1 to 3 hours.

[0017] Preferably, the first organic amine and the second organic amine are independently one or more of aliphatic amines, alcohol amines, amides, alicyclic amines and aromatic amines;

[0018] The mass ratio of the fluorinated graphene / metal oxide composite nanomaterial to the first organic amine is 1:0.5-30.

[0019] Preferably, the fatty amine is one or more of ethylenediamine, tert-butylamine, trimethylamine, n-butylamine, hexylamine and dodecylamine;

[0020] The alcoholamine is monoethanolamine and / or diethanolamine;

[0021] The amide is formamide and / or acetamide;

[0022] The alicyclic amine is triethylenediamine and / or diethylenetriamine;

[0023] The aromatic amine is diphenylamine and / or o-phenylenediamine.

[0024] Preferably, the amination treatment time is 0.5 to 4 hours;

[0025] The heating temperature of the amination-treated substrate is 30 to 120° C.

[0026] The film forming method is one or more of spraying, spin coating and electrodeposition.

[0027] The present invention provides a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating prepared by the above preparation method, wherein the components of the composite coating include fluorinated graphene / metal oxide composite nanomaterials and organic amine.

[0028] The present invention provides application of the above-mentioned fluorinated graphene / metal oxide nanoparticle / organic amine composite coating in the field of lubrication and / or corrosion protection.

[0029] The invention provides a method for preparing a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating, comprising the following steps: mixing a fluorinated graphene nanosheet (FG) alcohol dispersion and a metal oxide nanoparticle alcohol dispersion, and performing a solvothermal reaction under ultrasonic conditions to obtain a fluorinated graphene / metal oxide composite nanomaterial; mixing the fluorinated graphene / metal oxide composite nanomaterial, a first organic amine and an alcohol solvent to obtain a film-forming liquid; mixing a metal substrate with a second organic amine liquid, performing an amination treatment, and obtaining an amination-treated substrate; and forming a film of the film-forming liquid on the surface of the amination-treated substrate to obtain a fluorinated graphene / oxide nanoparticle / organic amine composite coating. The CF bond in FG has strong selective adsorption for the CH bond in organic molecules, so the van der Waals force of FG can be enhanced by introducing organic molecules between FG nanosheets and on the surface of the metal substrate. In addition, the CF bond in FG will be activated in an alkaline medium, especially under the action of organic amines, FG shows a high reactivity and can be covalently bonded with amino groups. Therefore, the present invention introduces organic amines between FG sheets and grafts organic amines on the surface of the metal substrate. By initiating a nucleophilic substitution reaction and with the help of the bridging effect of organic amines, covalent bonding between the substrate and the FG nanosheets and between the FG nanosheets can be achieved, thereby improving the stability of the fluorinated graphene coating.

[0030] Normally, a coating material constructed of a single two-dimensional nanomaterial will inevitably introduce structural defects such as holes and grain boundaries during the coating preparation process. These defects will cause the lubrication effect of the protective coating to be unstable or even fail to protect during the protection process. The present invention introduces zero-dimensional metal oxide nanoparticles into the two-dimensional fluorinated graphene nanosheet system, and the two can construct a multi-dimensional coupled nanocomposite structure to play a synergistic lubrication effect, thereby further improving its wear resistance without affecting the extreme pressure lubrication performance of FG. In addition, the metal oxide nanoparticles play a role in inhibiting the cathode corrosion of the substrate in acidic media. Therefore, the present invention can further enhance the lubrication and corrosion resistance of the composite coating by introducing metal oxide nanoparticles into the composite coating, and show a better service life in the atmospheric environment. It has great application potential in the construction of new functional lubricating coatings and long-life tribological service conditions. The results of the embodiment show that the friction coefficient of the fluorinated graphene / metal oxide nanoparticle / organic amine composite coating obtained by the present invention is 0.10-0.11, the lubrication life is 10300-12000 cycles, the corrosion voltage is -0.27-0.35 V, and the corrosion current is 1.2×10 -6 ~2.1×10 -6 A.cm -2 .

[0031] At the same time, the present invention adopts an ultrasound-assisted solvothermal method to prepare fluorinated graphene / metal oxide composite nanomaterials, combined with a simple amination treatment and film-forming process, the overall operation is simple, the cost is low, and it is easy to realize industrial mass production. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 FG / CeO 2 Microscopic morphology of nanocomposites;

[0033] Figure 2 FG / CeO 2 X-ray diffraction patterns and infrared spectra of nanocomposites;

[0034] Figure 3 Surface morphology of different coatings;

[0035] Figure 4 This is the Raman structure of the FG-EDA coating;

[0036] Figure 5 The lubrication performance under different ratios of FG and EDA;

[0037] Figure 6 Lubrication performance of composite coatings and single coatings;

[0038] Figure 7 FG / CeO2 - Lubrication performance of EDA coating under different loads;

[0039] Figure 8 The electrochemical test results of the composite coating and the control sample. DETAILED DESCRIPTION

[0040] The present invention provides a method for preparing a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating, comprising the following steps:

[0041] The fluorinated graphene nanosheet alcohol dispersion and the metal oxide nanoparticle alcohol dispersion are mixed, and a solvothermal reaction is carried out under ultrasonic conditions to obtain a fluorinated graphene / metal oxide composite nanomaterial;

[0042] Mixing the fluorinated graphene / metal oxide composite nanomaterial, a first organic amine and an alcohol solvent to obtain a film-forming solution;

[0043] The metal substrate is mixed with a second organic amine liquid and subjected to an amination treatment to obtain an amination-treated substrate;

[0044] The film-forming liquid is made to form a film on the surface of the amination-treated substrate to obtain a fluorinated graphene / oxide nanoparticle / organic amine composite coating.

[0045] Unless otherwise specified, the raw materials used in the present invention are all commercially available.

[0046] The present invention mixes a fluorinated graphene nanosheet alcohol dispersion and a metal oxide nanoparticle alcohol dispersion, and performs a solvothermal reaction under ultrasonic conditions to obtain a fluorinated graphene / metal oxide composite nanomaterial. In the present invention, the carbon-fluorine atomic ratio of the fluorinated graphene nanosheet is preferably 1.05 to 1.8, more preferably 1.2 to 1.6, and the average sheet diameter is preferably 5 to 40 μm.

[0047] In the present invention, the method for preparing the fluorinated graphene nanosheet alcohol dispersion preferably comprises the following steps:

[0048] The fluorinated graphene nanosheets and the alcohol solvent are ultrasonically mixed to obtain a fluorinated graphene nanosheet alcohol dispersion.

[0049] In the present invention, the alcohol solvent is preferably ethanol. In the present invention, the frequency of the ultrasonic mixing is preferably 40 kHz, and the time is preferably 10 to 240 min.

[0050] In the present invention, the mass concentration of the fluorinated graphene nanosheet alcohol dispersion is preferably 0.1 to 5 mg / mL.

[0051] In the present invention, the metal oxide is preferably MoO 3 、MgO、CeO2 、ZrO 2 , CuO and Y 2 O 3 One or more of the following; the particle size of the metal oxide nanoparticles is preferably 10 to 80 nm, more preferably 30 to 50 nm.

[0052] In the present invention, the method for preparing the metal oxide nanoparticle alcohol dispersion preferably comprises the following steps:

[0053] The metal oxide nanoparticles are mixed with an alcohol solvent to obtain an alcohol dispersion of the metal oxide nanoparticles.

[0054] In the present invention, the alcohol solvent is preferably ethanol. In the present invention, the mixing method is preferably stirring and mixing. In the present invention, the mass concentration of the metal oxide nanoparticle alcohol dispersion is preferably 0.1 to 3 mg / mL.

[0055] In the present invention, the mass ratio of the metal oxide nanoparticles to the fluorinated graphene nanosheets is preferably 1:4 to 20, more preferably 1:8 to 15. In the present invention, the mixing method of the fluorinated graphene nanosheet alcohol dispersion and the metal oxide nanoparticle alcohol dispersion is preferably stirring mixing, and more preferably magnetic stirring mixing. In the present invention, during the mixing, the metal oxide nanoparticle alcohol dispersion is preferably added dropwise to the fluorinated graphene nanosheet alcohol dispersion.

[0056] In the present invention, the solvent thermal reaction is preferably carried out in a high pressure reactor. In the present invention, the temperature of the solvent thermal reaction is preferably 80 to 160°C, more preferably 100 to 120°C; the time is preferably 0.1 to 3 hours, more preferably 1 to 2 hours. In the present invention, during the solvent thermal reaction, the speed of the high pressure reactor is preferably 100 to 2000 r / min, more preferably 500 to 1000 r / min.

[0057] After the solvothermal reaction, the present invention preferably performs post-treatment on the obtained solvothermal reaction liquid, and the post-treatment preferably comprises the following steps:

[0058] The solvent thermal reaction liquid is sequentially subjected to solid-liquid separation, washing and drying to obtain fluorinated graphene / metal oxide composite nanomaterial particles.

[0059] In the present invention, the solid-liquid separation is preferably suction filtration, and the filter paper used in the suction filtration is preferably 0.42 μm filter paper. In the present invention, the detergent used in the washing is preferably ethanol; and the drying is preferably freeze drying.

[0060] The present invention mixes the fluorinated graphene / metal oxide composite nanomaterial, the first organic amine and an alcohol solvent to obtain a membrane-forming solution. In the present invention, the first organic amine is preferably one or more of aliphatic amines, alcohol amines, amides, alicyclic amines and aromatic amines; in the present invention, the aliphatic amine is preferably one or more of ethylenediamine, tert-butylamine, trimethylamine, n-butylamine, hexylamine and dodecylamine; the alcohol amine is preferably monoethanolamine and / or diethanolamine; the amide is formamide and / or acetamide; the alicyclic amine is preferably triethylenediamine and / or diethylenetriamine; the aromatic amine is preferably diphenylamine and / or o-phenylenediamine.

[0061] In the present invention, the first organic amine is preferably a fatty amine.

[0062] In the present invention, the mass ratio of the fluorinated graphene / metal oxide composite nanomaterial to the first organic amine is preferably 1:0.5-30, more preferably 1:1-20, and further preferably 1:5-15.

[0063] In the present invention, the alcohol solvent is preferably ethanol.

[0064] In the present invention, the mixing method is preferably:

[0065] Firstly, the fluorinated graphene / metal oxide composite nanomaterial is ultrasonically mixed with an alcohol solvent, and then the first organic amine is added and stirred for mixing.

[0066] In the present invention, in the film-forming solution, the mass concentration of the fluorinated graphene / metal oxide composite nanomaterial is preferably 1 to 3 mg / mL, more preferably 2 mg / mL.

[0067] The present invention mixes a metal substrate with a second organic amine liquid and performs an amination treatment to obtain an amination-treated substrate. In the present invention, the second organic amine is preferably one or more of aliphatic amines, alcohol amines, amides, alicyclic amines and aromatic amines; in the present invention, the aliphatic amine is preferably one or more of ethylenediamine, tert-butylamine, trimethylamine, n-butylamine, hexylamine and dodecylamine; the alcohol amine is preferably monoethanolamine and / or diethanolamine; the amide is formamide and / or acetamide; the alicyclic amine is preferably triethylenediamine and / or diethylenetriamine; the aromatic amine is preferably diphenylamine and / or o-phenylenediamine.

[0068] In the present invention, the material of the metal substrate is preferably one or more of stainless steel, aluminum, and copper.

[0069] In the present invention, the mixing method is preferably to immerse the metal substrate in the second organic amine liquid. In the present invention, the temperature of the amination treatment is preferably room temperature, and the time is preferably 0.5 to 4 hours, more preferably 2 hours. In the process of the amination treatment, a complex reaction occurs on the surface of the metal substrate, thereby generating amino groups on the metal substrate, preparing for the next step of spraying.

[0070] The present invention allows the film-forming liquid to form a film on the surface of the amino-treated substrate to obtain a fluorinated graphene / oxide nanoparticle / organic amine composite coating. In the present invention, the film-forming method is preferably one or more of spraying, spin coating and electrodeposition; in the present invention, the spraying is preferably high-purity nitrogen spraying, and the spraying pressure is preferably 0.2-0.6MPa; the spin coating speed of the spin coating is preferably 1000r / min, the time is preferably 30s, and the number of spin coatings is preferably multiple times; in the present invention, the voltage of the electrodeposition is preferably 20-45V, more preferably 25-40V, further preferably 30-35V, and the time is preferably 1.5h.

[0071] During the film formation, the present invention preferably heats the amino treated substrate, and the heating temperature is preferably 30 to 120° C., more preferably 60 to 100° C. In the present invention, the heating serves to cure and accelerate the film formation.

[0072] The present invention provides a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating prepared by the above preparation method, wherein the components of the composite coating include fluorinated graphene / metal oxide composite nanomaterials and organic amine.

[0073] The present invention provides application of the above-mentioned fluorinated graphene / metal oxide nanoparticle / organic amine composite coating in the field of lubrication and / or corrosion protection.

[0074] The fluorinated graphene / metal oxide nanoparticle / organic amine composite coating provided by the present invention and its preparation method and application are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0075] The fluorinated graphene (FG) nanosheets used in the following examples have a carbon-fluorine ratio of 1.05 and an average sheet diameter of 20 μm, and are prepared by Shandong Chongshan Optoelectronic Materials Co., Ltd.;

[0076] Anhydrous ethanol from Sinopharm Chemical Reagent Co., Ltd. was used;

[0077] Homemade deionized water was used.

[0078] Example 1

[0079] Weigh 45 mg of fluorinated graphene (FG) raw material and add it into a beaker containing 45 mL of ethanol. After ultrasonic treatment for 30 min, a 1 mg / mL FG ethanol suspension is obtained. Weigh 5 mg CeO 2 The nanoparticles were added to a 10 mL beaker to prepare a 0.5 mg / mL nanoparticle ethanol solution. The beaker containing the FG ethanol dispersion was placed on a magnetic stirring table and continued to stir, and then the prepared nanoparticle dispersion was added dropwise within 20 min. After the addition was completed, the mixed solution was transferred to a high-pressure reactor for solvothermal reaction. The reaction conditions were set as follows: temperature 120 ° C, speed 500 r / min, time 2 h, and 40 kHz ultrasonic treatment. After the reaction was completed, a 0.42 μm filter paper was used for suction filtration, and it was repeatedly washed with ethanol. The obtained filter cake was freeze-dried to obtain the final FG / CeO 2 Composite nanomaterials.

[0080] The stainless steel sheet was immersed in dodecylamine for 1 h for amination and then taken out to prepare 2 mg / mL FG / CeO 2 The ethanol dispersion of the composite nanomaterial was ultrasonically mixed evenly, and then ethylenediamine was added and ultrasonicated for half an hour. 2 The mass ratio of ethylenediamine to 1:15 was 1.5 mL of the dispersion was sprayed on the surface of the amination-treated stainless steel sheet heated on a heating plate at 100 °C each time. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain FG / CeO 2 Composite coating.

[0081] Example 2

[0082] According to the method of Example 1, CeO 2 Nanoparticles replaced with ZrO 2 Nanoparticles, FG / ZrO 2 Composite nanomaterials.

[0083] The stainless steel sheet was immersed in triethylenediamine for amination treatment for 1 h and then taken out to prepare 2 mg / mL FG / ZrO 2 The ethanol dispersion was ultrasonically mixed evenly, and then o-phenylenediamine was added and ultrasonicated for half an hour. 2 The mass ratio of the dispersion to o-phenylenediamine was 1:10. 1.5 mL of the dispersion was sprayed on the surface of the amination-treated stainless steel sheet heated on a heating plate at 100 °C. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain FG / ZrO 2 Composite coating.

[0084] Example 3

[0085] According to the method of Example 1, CeO 2The nanoparticles are replaced with CuO nanoparticles to obtain FG / CuO composite nanomaterials.

[0086] The stainless steel sheet was immersed in dodecylamine for amination treatment for 1 hour and then taken out, a 2 mg / mL FG / CuO ethanol dispersion was prepared and ultrasonically mixed evenly, and tert-butylamine was added for half an hour of ultrasonication. The mass ratio of FG / CuO to tert-butylamine was 1:15. 1.5 mL of the dispersion was sprayed on the surface of the amination-treated stainless steel sheet heated at 100°C on a heating plate each time. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain a FG / CuO composite coating.

[0087] Example 4

[0088] Compared with Example 1, the heating temperature of the amination-treated stainless steel sheet is 80°C.

[0089] Example 5

[0090] Compared with Example 1, the heating temperature of the amination-treated stainless steel sheet is 120°C.

[0091] Example 6

[0092] Compared with Example 1, the mass ratio of metal oxide nanoparticles to fluorinated graphene nanosheets is 1:15.

[0093] Example 7

[0094] Compared with Example 1, the mass ratio of metal oxide nanoparticles to fluorinated graphene nanosheets is 1:10.

[0095] Comparative Example 1

[0096] The stainless steel sheet was immersed in dodecylamine for amination treatment for 1 hour and then taken out. A 2 mg / mL FG ethanol dispersion was prepared and ultrasonically mixed evenly. 1.5 mL of the dispersion was sprayed on the surface of the stainless steel sheet heated at 100°C on a heating plate each time. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain a FG-based coating.

[0097] Comparative Example 2

[0098] The stainless steel sheet was immersed in diethylenetriamine for amination treatment for 1 hour and then taken out. A 2 mg / mL FG ethanol dispersion was prepared and ultrasonically mixed evenly. Ethylenediamine was added and ultrasonically mixed for half an hour. The mass ratio of FG to ethylenediamine was 2:1. 1.5 mL of the dispersion was sprayed on the surface of the stainless steel sheet heated at 100°C on a heating plate each time. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain an FG-based composite coating 2-1.

[0099] Comparative Example 3

[0100] The stainless steel sheet was immersed in dodecylamine for amination treatment for 1 hour and then taken out, a 2 mg / mL FG ethanol dispersion was prepared and ultrasonically mixed evenly, and then tert-butylamine was added and ultrasonically mixed for half an hour. The mass ratio of FG to tert-butylamine was 1:1. Each time, 1.5 mL of the dispersion was sprayed on the surface of the stainless steel sheet heated at 100°C on a heating plate. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain an FG-based composite coating 1-1.

[0101] Comparative Example 4

[0102] The stainless steel sheet was immersed in tert-butylamine for amination treatment for 1 hour and then taken out, a 2 mg / mL FG ethanol dispersion was prepared and ultrasonically mixed evenly, and then ethylenediamine was added and ultrasonically mixed for half an hour. The mass ratio of FG to ethylenediamine was 1:3. Each time, 1.5 mL of the dispersion was sprayed on the surface of the stainless steel sheet heated at 100°C on a heating plate. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain FG / organic amine composite coatings 1-3.

[0103] Comparative Example 5

[0104] The stainless steel sheet was immersed in o-phenylenediamine for amination treatment for 1 hour and then taken out, a 2 mg / mL FG ethanol dispersion was prepared and ultrasonically mixed evenly, and then ethylenediamine was added and ultrasonically mixed for half an hour. The mass ratio of FG to ethylenediamine was 1:5. Each time, 1.5 mL of the dispersion was sprayed on the surface of the stainless steel sheet heated at 100°C on a heating plate. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain FG-based composite coatings 1-5.

[0105] Comparative Example 6

[0106] The stainless steel sheet was immersed in ethylenediamine for amination treatment for 1 hour and then taken out, a 2 mg / mL FG ethanol dispersion was prepared and ultrasonically mixed evenly, and then dodecylamine was added and ultrasonically mixed for half an hour. The mass ratio of FG to dodecylamine was 1:15. Each time, 1.5 mL of the dispersion was sprayed on the surface of the copper block heated at 100°C on a heating plate. The direction of the copper block was adjusted after each spraying. A total of 4 sprayings were performed to obtain FG-based composite coatings 1-15.

[0107] Comparative Example 7

[0108] The stainless steel sheet was immersed in ethylenediamine for amination treatment for 1 hour and then taken out, a 2 mg / mL FG ethanol dispersion was prepared and ultrasonically mixed evenly, and then o-phenylenediamine was added and ultrasonically mixed for half an hour. The mass ratio of FG to o-phenylenediamine was 1:30. Each time, 1.5 mL of the dispersion was sprayed on the surface of the stainless steel sheet heated at 100°C on a heating plate. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain an FG-based composite coating 1-30.

[0109] Comparative Example 8

[0110] The stainless steel sheet was immersed in dodecylamine for 1 h for amination and then taken out to prepare 2 mg / mL FG / CeO 2 The ethanol dispersion was ultrasonically mixed and sprayed directly. 1.5 mL of the dispersion was sprayed on the surface of the stainless steel sheet heated at 100° C. on a heating plate each time. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain a FG-based composite coating.

[0111] Comparative Example 9

[0112] Using untreated stainless steel sheets as substrate, 2 mg / mL FG / CeO 2 The ethanol dispersion was ultrasonically mixed evenly, and then tert-butylamine was added and ultrasonicated for half an hour. The mass ratio of FG to tert-butylamine was 1:10. 1.5 mL of the dispersion was sprayed on the surface of the stainless steel sheet heated at 100°C on a heating plate each time. The direction of the stainless steel sheet was adjusted after each spraying. A total of 4 sprayings were performed to obtain an FG-based composite coating.

[0113] Structural characterization

[0114] (1) FG / CeO 2 The microstructure of nanocomposite materials is shown in Figure 2. Figure 1 As shown by Figure 1 It can be seen that Figure 1 CeO in a 2 The particle size distribution of the nanoparticles is relatively narrow, and most of the nanoparticles have a particle size of about 20nm. The nanoparticles are basically octahedral structures; the lattice spacing of 0.32nm in HR-TEM corresponds to CeO 2 The (111) crystal plane of the crystal. 2 The ferromagnetism caused by its own crystal defects and the nanosize effect make it more likely to agglomerate than other nanoparticles. Figure 1 b is the TEM of FG, and the results show that FG is a few-layer structure with obvious wrinkles on the surface. The above results prove that the FG used in this study is a thin-layer two-dimensional nanosheet structure with good flexibility. Figure 1 c and d are FG / CeO 2 TEM and HR-TEM images of the nanocomposite material show that the FG nanosheets and CeO 2 Nanoparticles were successfully composited. CeO 2 The dispersion of nanoparticles on the surface of FG nanosheets has improved, but there is still some agglomeration, indicating that CeO 2 Nanoparticles have a certain adsorption capacity on FG sheets, but CeO 2 The adsorption between nanoparticles will lead to partial agglomeration on the surface of FG nanosheets. HR-TEM results show that CeO 2The octahedral structure of the nanoparticles has changed.

[0115] (2) FG / CeO 2 The X-ray diffraction patterns and infrared spectra of nanocomposites are shown in Figure 2. Figure 2 As shown, Figure 2 (a) is the X-ray diffraction diagram, and (b) is the infrared spectrum diagram. Figure 2 It can be seen that the XRD analysis of the raw material CeO 2 The crystal structures of FG and the prepared composite materials were characterized. Figure 2 a. CeO 2 The diffraction peaks of the XRD spectrum are consistent with the face-centered cubic structure of CeO 2 The characteristic peaks of the crystal, among which the main diffraction peaks at 28.6°, 33.1°, 47.5° and 56.4° correspond to CeO 2 Characteristic peaks of the (111) face, (200) face, (220) face and (311) face of the crystal. Two diffraction peaks located near 14° and 41° appeared in the XRD spectrum of FG, which correspond to the (001) face diffraction peak representing the interlayer spacing in high F content FGi and the (100) face diffraction peak representing the CC bond length in the six-membered ring unit of the carbon skeleton in FG. FG / CeO 2 The XRD diffraction peaks of the nanocomposite materials were consistent with the corresponding characteristic peaks in the raw materials, and there was no obvious shift, which proved that the lattice of the reactants was not affected under the set reaction conditions. 2 The chemical bond structure of the composite material was characterized. Figure 2 b. 1217cm -1 The singlet near 3400cm represents the characteristic peak of the stretching vibration of the CF bond in FG, while -1 The broad peak near represents the characteristic peak of OH bond stretching vibration; in the synthesis of FG / CeO 2 The strength and position of the CF bond did not change significantly during the composite nanomaterials, indicating that the chemical structure of FG was not affected during the solvothermal reaction. 2 Except for the characteristic peaks of CeO, no new characteristic peaks were found in the FT-IR graph of the composite material. 2 The modification of FG is a physical process and no chemical reaction occurs.

[0116] (3) Surface morphology of different coatings Figure 3 As shown, Figure 3 (a) pure CeO 2 Coatings, (b) is the original FG coating, (c) is FG / CeO 2Coatings, (d) is FG-EDA coating, (e, f) are FG / CeO 2 -EDA coating. Figure 3 It can be seen that pure CeO 2 The surface of the coating is relatively smooth, while the surface of the pure FG coating has more particles and the particle size is larger. The low surface energy of FG makes it difficult for it to form a complete film on the surface of the substrate, so it accumulates on the surface of the substrate in the form of particles. 2 The surface morphology of the composite coating did not change significantly, indicating that the addition of CeO 2 The film-forming ability of FG was not improved. The surface of FG-EDA coating was significantly smoother than that of pure FG coating, indicating that EDA affected the interfacial bonding behavior of FG. Figure 3 As shown in e and f, FG / CeO 2 The surface of the -EDA composite coating is also very smooth with only a small amount of particles.

[0117] (4) Raman structure of FG-EDA coating Figure 4 As shown. Figure 4 It can be seen that with the increase of EDA ratio, the I D / I G The value gradually increases. This shows that as the proportion of EDA increases, the internal structure of the FG coating will be damaged to varying degrees, thus affecting the physical and chemical properties of FG.

[0118] Performance Testing

[0119] (1) Lubrication performance and service life of composite coating and comparative example

[0120] Using TRB 3 The tribological properties of water-based lubricants were characterized by the reciprocating ball-on-disk motion mode of a friction tester (Anton Paar, Switzerland). The friction pair consisted of a GCr15 steel ball with a diameter of 6 mm and a stainless steel block polished with 1000 grit sandpaper. The lubrication performance and wear life of the coating were mainly investigated. The load was 20 N, the reciprocating stroke was 6 mm, the frequency was 1 Hz, and the test was carried out in an atmospheric environment. Each sample was subjected to more than 3 friction tests to eliminate errors in the preparation and testing process.

[0121] Lubrication performance under different ratios of FG and EDA Figure 5 As shown. Figure 5It can be seen that compared with pure FG coating, the addition of EDA can significantly improve the lubrication life of the coating, but has little effect on the friction coefficient of the coating. This is because EDA improves the interfacial bonding behavior of FG through its own amino group, and good bonding is the key to improving the lubrication life of FG coating, and it does not directly lubricate itself. Among them, when the ratio of FG to EDA is 1:10, the coating shows the best lubrication life.

[0122] Lubrication performance of composite coating and single coating Figure 6 As shown. Figure 6 It can be seen that the friction coefficient of the original stainless steel substrate is very high, reaching 0.68. After spraying the coating on its surface, the friction coefficient is significantly reduced; pure CeO 2 The friction coefficient of the coating is higher than 0.2, and it fails quickly in a very short time; the friction coefficient of the pure FG coating is about 0.1, and it fails after 3000 cycles; FG and CeO 2 After direct compounding, the lubrication life and friction coefficient did not change significantly, indicating that CeO 2 The direct introduction of EDA failed to play an improvement role. However, it was found that as EDA was introduced into the coating, the lubrication life of the corresponding coating increased exponentially. This is mainly because EDA improved the interfacial bonding behavior of FG, thereby improving the mechanical properties and substrate bonding strength of the FG composite coating, both of which play an important role in the lubrication performance of the FG coating. 2 The -EDA composite coating exhibits the best lubrication performance, with a lubrication life three times longer than that of pure FG coating and a life of 3,000 cycles longer than that of FG-EDA coating.

[0123] FG / CeO 2 -Lubrication performance of EDA coating under different loads Figure 7 As shown. Figure 7 It can be seen that as the load increases, the friction coefficient of the coating decreases slightly, and although the lubrication life varies, it basically remains above 11,000 cycles. Through analysis, it is found that as the load increases, the running-in time of the coating is shortened, but the coating fails faster. This may be because large loads make it easier to form a lubricating film, but it is also easier to destroy lubrication and cause coating failure.

[0124] (2) Electrochemical corrosion performance of composite coating and comparative example

[0125] The surface coating of the stainless steel substrate was tested by potentiodynamic polarization curve and electrochemical impedance spectroscopy using a CHI660E electrochemical workstation. A 3.5wt.% NaCl aqueous solution was selected as the corrosion medium, and a traditional three-electrode system was used, namely, bare stainless steel and coated stainless steel electrodes as working electrodes, Ag / AgCl electrodes (filled with 3.5M KCl) as reference electrodes, and platinum electrodes as auxiliary electrodes. After connecting the electrodes, the electrode system was stabilized by running the open circuit potential, and then the system was subjected to an electrochemical impedance spectroscopy test. The test conditions selected the interference signal amplitude of 0.01V and the frequency range of 10mHz to 100kHz. The electrochemical impedance spectroscopy data were fitted and analyzed using ZSimpWin software. After that, the system was subjected to a potentiodynamic polarization curve test. During the test, the scanning speed was 1mV / s and the scanning range was -1V to 1V. The electrochemical tests under the same conditions were repeated at least 3 times to ensure the repeatability of the experiment, and representative experimental results were selected.

[0126] The electrochemical test results of the composite coating and the comparison sample are as follows Figure 8 As shown. Figure 8 It can be seen that the corrosion potential of stainless steel is -0.51V and the corrosion current density is 4.9×10 -6 A.cm -2 Compared with the bare stainless steel substrate, the corrosion current density of the FG composite coating and the single material coating is reduced, indicating that these coatings have slowed down the corrosion of the corrosive medium on the stainless steel substrate and have a certain corrosion resistance on the substrate. 2 Although the coating has a certain degree of corrosion protection for stainless steel, the protection performance is very weak. However, after the two are combined, the corrosion potential of the coating becomes more positive and the corresponding corrosion current is reduced accordingly. 2 There is a synergistic effect, which more effectively prevents the corrosive medium from invading the substrate surface. Compared with the pure FG coating, the anti-corrosion performance of the FG inner coating is significantly improved with the introduction of EDA. On the one hand, EDA covalently bonds with FG, making it more tightly bonded to the stainless steel substrate, making it difficult for the corrosive medium to invade. On the other hand, EDA itself can be adsorbed on the substrate surface as a corrosion inhibitor, thereby further slowing down the destructiveness of the infiltrated corrosive medium to the substrate.

[0127] The performance test results of the coatings obtained in the examples and comparative examples are shown in Tables 1 and 2.

[0128] Table 1 Performance test results of the coating obtained in Example

[0129]

[0130] Table 2 Performance test results of the coating obtained in the comparative example

[0131]

[0132]

[0133] It can be seen from Tables 1 and 2 that the method provided by the present invention can construct a stable fluorinated graphene-based composite coating, and the obtained fluorinated graphene / metal oxide nanoparticles / organic amine composite coating has excellent lubrication and corrosion resistance.

[0134] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating, comprising the following steps: The fluorinated graphene nanosheet alcohol dispersion and the metal oxide nanoparticle alcohol dispersion are mixed, and a solvothermal reaction is carried out under ultrasonic conditions to obtain a fluorinated graphene / metal oxide composite nanomaterial; the metal oxide is one or more of MoO3, MgO, CeO2, ZrO2, CuO and Y2O3; Mixing the fluorinated graphene / metal oxide composite nanomaterial, a first organic amine and an alcohol solvent to obtain a film-forming solution; The metal substrate is mixed with a second organic amine liquid and subjected to an amination treatment to obtain an amination-treated substrate; The film-forming liquid is made to form a film on the surface of the heated amination-treated substrate to obtain a fluorinated graphene / metal oxide nanoparticle / organic amine composite coating.

2. The preparation method according to claim 1, characterized in that: The carbon-fluorine atomic ratio of the fluorinated graphene nanosheet is 1.05-1.8, and the average sheet diameter is 5-40 μm.

3. The preparation method according to claim 1, characterized in that: The particle size of the metal oxide nanoparticles is 10 to 80 nm.

4. The preparation method according to any one of claims 1 to 3, characterized in that: The mass ratio of the metal oxide nanoparticles to the fluorinated graphene nanosheets is 1:4-20.

5. The preparation method according to claim 1, characterized in that: The temperature of the solvent thermal reaction is 80-160° C., and the time is 0.1-3 hours.

6. The preparation method according to claim 1, characterized in that: The first organic amine and the second organic amine are independently one or more of aliphatic amines, alcohol amines, amides, alicyclic amines and aromatic amines; The mass ratio of the fluorinated graphene / metal oxide composite nanomaterial to the first organic amine is 1:0.5-30.

7. The preparation method according to claim 6, characterized in that: The fatty amine is one or more of ethylenediamine, tert-butylamine, trimethylamine, n-butylamine, hexylamine and dodecylamine; The alcoholamine is monoethanolamine and / or diethanolamine; The amide is formamide and / or acetamide; The alicyclic amine is triethylenediamine and / or diethylenetriamine; The aromatic amine is diphenylamine and / or o-phenylenediamine.

8. The preparation method according to claim 1 or 6, characterized in that: The amination treatment time is 0.5 to 4 hours; The heating temperature of the amination-treated substrate is 30 to 120° C. The film forming method is one or more of spraying, spin coating and electrodeposition.

9. A fluorinated graphene / metal oxide nanoparticle / organic amine composite coating prepared by the preparation method according to any one of claims 1 to 8, wherein the components of the composite coating include fluorinated graphene / metal oxide composite nanomaterials and organic amine.

10. Use of the fluorinated graphene / metal oxide nanoparticle / organic amine composite coating according to claim 9 in the field of lubrication and / or corrosion protection.