A composite catalyst and its preparation and application

By loading iron-tungstate on kaolin to form composite catalysts, the problems of environmental pollution and high catalyst costs in traditional plastic film recycling and reuse are solved, efficient and low-cost resource utilization are achieved, and the pyrolysis conversion rate and fuel of plastic film are improved. Oil production.

CN116713004BActive Publication Date: 2024-11-22FUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310736460.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-21
Publication Date
2024-11-22
Estimated Expiration
2043-06-21

AI Technical Summary

Technical Problem

Traditional plastic film recycling and reuse methods lead to environmental pollution, and the existing catalysts are costly, poor repeatability, and low pyrolysis efficiency, making it difficult to achieve efficient resource utilization.

Method used

The composite catalyst of ferrotungstate and kaolin is used to form Lewis acid sites and Bronst acid sites by supporting ferrotungstate on kaolin, which is used to catalyze pyrolysis of mulch film, reduce the pyrolysis temperature and time, and improve the conversion rate.

Benefits of technology

It realizes a low-cost and easy-to-recycle catalyst, improves the conversion rate of plastic film pyrolysis, and has a high fuel oil content within the C5-C12 range in the product, which saves energy consumption, and is suitable for large-scale plastic film industry catalytic pyrolysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116713004B_ABST
    Figure CN116713004B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of waste mulch film catalytic pyrolysis resource utilization, and more specifically relates to a method for preparing a low-cost iron tungstate / kaolin composite catalyst and its application in the catalytic pyrolysis process of mulch film. First, iron salt and tungstate are mixed under certain conditions to prepare iron tungstate K6[H2FeBW 11 O 40 ]·9H2O, and then the iron tungstate solution is added dropwise in a certain proportion to a system in which kaolin and water are uniformly dispersed to react to obtain an iron tungstate / kaolin composite catalyst, and applied to the catalytic pyrolysis process of ground film to obtain liquid oil and gas products with a total yield of up to 96.9%, wherein the content of fuel oil in the C5-C12 range can be as high as 52% or more. The present invention has the characteristics of low energy consumption, high ground film cracking conversion rate, and great industrialization potential, meets the requirements of developing renewable resources, developing a green circular economy, and taking the path of sustainable development, broadens the way to utilize resources after ground film recovery, and has very important economic benefits, social benefits and environmental benefits.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of resource utilization of catalytic cracking of ground film, and more specifically to a composite catalyst and its preparation and application in catalytic thermal cracking of waste ground film. Background Art

[0002] Plastic mulch is an important auxiliary material for agricultural production in arid areas. It has the functions of heat preservation and moisture retention, weed suppression, ground temperature increase, and yield increase. It is widely used in the arid northwest and cold northeast regions. As a major agricultural producer, my country uses a very high amount of mulch. If a large amount of mulch is not recycled in time after use, it will remain in the soil and difficult to degrade, which will cause a series of pollution to the environment. Therefore, it is necessary to regularly recycle and reuse the waste mulch. The traditional recycling and reuse method is to manually collect and pack the mulch and transport it to the power plant for combustion and power generation. This treatment method causes the mulch to produce a large amount of harmful gases during the combustion process, which causes serious pollution to the environment. In addition, some mulch recycling methods use traditional pyrolysis devices to oil or gasify waste mulch, but the oil and gas production of the process is low, and the oil and gas production types are more, the selectivity is low, and the pyrolysis efficiency is not high. Therefore, how to efficiently catalyze the pyrolysis of waste mulch for resource utilization has become a key issue that needs to be solved.

[0003] Introducing a catalyst during the pyrolysis process is a common solution. Zeolite has become a widely used catalyst due to its strong acid resistance, favorable carbon-carbon bond breaking, and good catalytic performance for polymer degradation. However, the small pore size of zeolite hinders the contact between the bulky polymer chains and the acid sites located in the pores, and the carbon deposition during the pyrolysis process will cause it to deactivate rapidly. In order to overcome this problem, people began to study the incorporation of some metal ions and heteropoly acids into the silicon framework to improve the catalytic performance, but the existing technology still has the problems of high cost, poor repeatability, low conversion rate of pyrolysis products of land film, and a sharp decrease in catalytic performance after recovery. Summary of the invention

[0004] To this end, it is necessary to provide a composite catalyst and its preparation and application, so as to obtain a catalyst with lower cost, higher efficiency, easy recycling and good secondary recovery catalytic performance, and use it to improve the catalytic pyrolysis of polyethylene mulch into light fuel oil and organic gas, so as to achieve the purpose of effectively realizing the resource utilization of waste mulch.

[0005] To achieve the above object, in a first aspect of the present invention, the inventor provides a method for preparing a composite catalyst, comprising the following steps:

[0006] Tungstate, water and boric acid are mixed in a certain mass ratio, reacted at a certain pH value and a certain temperature to obtain a reaction mixture system, allowed to stand, and the precipitate is removed to obtain a reaction mixture solution;

[0007] Adding the trivalent iron salt solution dropwise into the reaction mixture, reacting at a certain pH value and a certain temperature, cooling to room temperature, adding potassium salt and mixing evenly, separating and removing solid matter, washing, and obtaining iron tungstate;

[0008] The kaolin and water are uniformly mixed in a certain mass ratio, a certain mass fraction of tungstate iron solution is added dropwise, and the mixture is placed in a water bath for reaction to obtain the composite catalyst.

[0009] In a preferred embodiment of the present invention, the mass ratio of the tungstate, water and boric acid is 5 to 10:20:1. Tungstate can be a salt formed by ammonium ions, alkali metals, alkaline earth metals and many heavy metal cations with tungstate or polytungstate. Considering the production cost and reaction activity, sodium tungstate or calcium tungstate is preferred. More preferably, using boiling water or deionized water with a temperature close to 100°C will greatly increase the dissolution rate of tungstate and shorten the reaction time.

[0010] In a preferred embodiment of the present invention, the mass ratio of kaolin and water is 1 to 3:20, the mass fraction of the ferrotungstate solution is 10% to 50%, and the mass ratio of the potassium salt to boric acid is 2 to 3:1. The ferrotungstate solution, kaolin and water react in such a ratio under the action of the potassium salt and boric acid in the above mass ratio, so that the ferrotungstate can obtain a better loading effect on the kaolin, that is, the obtained composite catalyst can obtain more Lewis acid sites and Bronsted acid sites to improve the catalytic pyrolysis performance.

[0011] In some preferred embodiments, the pH values ​​of the steps of obtaining the reaction mixture system and obtaining the ferrotungstate are both 6 to 7. The pH value can be adjusted by, for example, one or a mixture of two or more of glacial acetic acid, citric acid, phosphoric acid, salicylic acid, sulfuric acid, aminosulfonic acid, phosphoric acid, gluconic acid, tartaric acid, succinic acid, and maleic acid with appropriate mass fractions. Preferably, the reaction temperature of the steps of obtaining the reaction mixture system and obtaining the ferrotungstate is both 80°C to 90°C.

[0012] In a preferred embodiment of the present invention, the temperature of the reaction mixture after standing is 0°C to 10°C, and the standing time is 12h to 36h. More preferably, when the ferrotungstate solution, kaolin and water are mixed and reacted in a water bath, the temperature of the water bath is 60°C to 80°C.

[0013] In the second aspect of the present invention, the inventor provides a composite catalyst prepared by the preparation method provided in the first aspect of the present invention. The mass fraction of iron tungstate in the composite catalyst is 10% to 50%.

[0014] In the third aspect of the present invention, the inventor provides a method for catalytically pyrolyzing a ground film using the composite catalyst provided in the second aspect of the present invention, comprising the following steps:

[0015] The composite catalyst and the ground film are mixed at a mass ratio of 10 to 27.6:1, placed in a pyrolysis reactor, and heated for a certain period of time in an inert gas environment.

[0016] Preferably, the heating reaction temperature is 350°C to 400°C.

[0017] In the fourth aspect of the present invention, the inventor provides a fuel oil obtained by catalytic pyrolysis of a ground film using the composite catalyst provided in the second aspect of the present invention, wherein the fuel oil contains a large amount of organic matter in the C5-C12 range.

[0018] In the fifth aspect of the present invention, the inventor provides a recovered gas obtained by catalytically pyrolyzing a ground film using the composite catalyst provided in the second aspect of the present invention.

[0019] Different from the prior art, the above technical solution has the following beneficial effects:

[0020] 1. The present invention provides a method for preparing a composite catalyst, by loading tungstate iron on kaolin, so that sufficient Lewis acid sites and Bronsted acid sites are generated on the catalyst to improve its catalytic pyrolysis performance, thereby achieving the purpose of simply, efficiently and cost-effectively producing a composite catalyst with stable catalytic performance, good repeatability and good recycling effect.

[0021] 2. Compared with traditional mulch film pyrolysis catalysts, the composite catalyst provided by the present invention effectively reduces the cracking temperature and reaction time of the mulch film, thereby reducing the energy required in the pyrolysis process. At the same time, the use of relatively low-priced kaolin as a catalyst raw material greatly saves the cost of resource utilization of mulch film cracking. In addition, the inventors found that the composite catalyst is easy to recycle, has good thermal stability, and has stable catalytic performance after recycling. It can be recycled for multiple times in mulch film pyrolysis, which solves the defects of traditional catalysts that are difficult to recycle or have greatly reduced catalytic performance after recycling, and is expected to be applied to large-scale industrial catalytic pyrolysis processes of mulch films.

[0022] 3. The present invention applies the composite catalyst to catalytic pyrolysis of mulch film. Based on the synergistic effect of a large number of Lewis acid sites and Bronsted acid sites, the cracking conversion rate is greatly improved, and the conversion rate can reach up to 96.9%. At the same time, by shortening the reaction time, the secondary reaction to produce aromatic compounds is prevented, which greatly improves the yield of light hydrocarbon fuel oil and organic gas after catalytic pyrolysis of mulch film, wherein the content of fuel oil in the range of C5-C12 can be as high as 52% or more.

[0023] In summary, the present invention first prepares iron tungstate K6[H2FeBW by mixing iron salt and tungstate under certain conditions. 11 O 40 ]·9H2O, and then add the ferrotungstate solution dropwise in a certain proportion to a system in which kaolin and water are evenly dispersed to react to obtain a low-cost ferrotungstate / kaolin composite catalyst, which is applied to the catalytic pyrolysis of mulch to obtain a large amount of liquid oil with fuel value. A ferrotungstate / kaolin composite catalyst with low cost, excellent catalytic performance, easy recovery and multiple recycling has been developed, and is applied to catalytic cracking of mulch to obtain liquid oil in the fuel range (C5-C12). It has the characteristics of low energy consumption, high cracking conversion rate and great industrialization potential, meets the requirements of developing renewable resources, developing a green circular economy and taking the path of sustainable development, broadens the way of resource utilization after mulch recovery, provides an ecological and environmentally friendly scientific and technological innovation idea for industrial catalytic pyrolysis of mulch, and provides a technical reference for the realization of energy conservation, emission reduction and resource recycling, and has very important economic, social and environmental benefits.

[0024] The above-mentioned records related to the invention content are only an overview of the technical solution of the present application. In order to enable ordinary technicians in the field to more clearly understand the technical solution of the present application, and then implement it according to the text of the specification and the contents recorded in the drawings, and to make the above-mentioned purpose and other purposes, features and advantages of the present application easier to understand, the following is an explanation in combination with the specific implementation mode and drawings of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a SEM image of a 10% by mass tungstate iron / kaolin composite catalyst provided in Example 1 of the present invention;

[0026] Figure 2 This is a SEM image of a 30% by mass tungstate iron / kaolin composite catalyst provided in Example 3 of the present invention;

[0027] Figure 3 This is a SEM image of a 50% by mass tungstate iron / kaolin composite catalyst provided in Example 5 of the present invention. DETAILED DESCRIPTION

[0028] In order to explain the technical content, structural features, achieved objectives and effects of the technical solution in detail, the following is a detailed description in conjunction with specific embodiments and accompanying drawings.

[0029] Reference to "embodiment" herein means that the specific features, structures or characteristics described in conjunction with the embodiment may be included in at least one embodiment of the present application. The term "embodiment" appearing in various places in the specification does not necessarily refer to the same embodiment, nor does it particularly limit its independence or association with other embodiments. In principle, in the present application, as long as there is no technical contradiction or conflict, the various technical features mentioned in the embodiments can be combined in any way to form a corresponding implementable technical solution.

[0030] Unless otherwise defined, the technical terms used in this document have the same meanings as those generally understood by those skilled in the art to which this application belongs; the use of relevant terms in this document is only for describing specific embodiments and is not intended to limit this application.

[0031] In the description of this application, the term "and / or" is an expression used to describe the logical relationship between objects, indicating that three relationships may exist, for example, A and / or B, which means: A exists, B exists, and A and B exist at the same time. In addition, the character " / " in this article generally indicates that the objects before and after are in an "or" logical relationship.

[0032] In the present application, terms such as “first” and “second” are merely used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any actual relationship of quantity, priority or sequence between these entities or operations.

[0033] Without further limitations, in this application, the words "include", "comprises", "has" or other similar expressions used in the sentences are intended to cover non-exclusive inclusion. These expressions do not exclude the presence of additional elements in the process, method or product including the elements, so that the process, method or product including a series of elements may include not only those limited elements, but also other elements not explicitly listed, or also include elements inherent to such process, method or product.

[0034] Similar to the understanding in the Examination Guidelines, in this application, expressions such as "greater than", "less than", "exceed" and the like are understood to exclude the number itself; expressions such as "above", "below", "within" and the like are understood to include the number itself. In addition, in the description of the embodiments of this application, "multiple" means more than two (including two), and similar expressions related to "multiple" are also understood in this way, such as "multiple groups", "multiple times", etc., unless otherwise clearly and specifically limited.

[0035] In the description of the embodiments of the present application, space-related expressions used, such as "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "vertical", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicate the orientation or position relationship based on the orientation or position relationship shown in the specific embodiments or drawings, and are only for the convenience of describing the specific embodiments of the present application or facilitating the reader's understanding, and do not indicate or imply that the referred device or component must have a specific position, a specific orientation, or be constructed or operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present application.

[0036] Unless otherwise expressly specified or limited, in the description of the embodiments of the present application, the terms such as "install", "connect", "connect", "fix", "set", etc. used should be understood in a broad sense. For example, the "connection" can be a fixed connection, a detachable connection, or an integrated setting; it can be a mechanical connection, an electrical connection, or a communication connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium; it can be the internal connection of two elements or the interaction relationship between two elements. For technicians in the technical field to which the present application belongs, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0037] The use of plastic mulch, an important material for agricultural production in arid areas, has contributed to increasing agricultural production and income, but it has also brought a considerable burden to the ecological environment. The current common way to recycle and reuse mulch is to collect and pack the mulch manually and transport it to power plants for combustion and power generation. This treatment method causes the mulch to produce a large amount of harmful gases during the combustion process, causing serious secondary pollution to the environment. Other methods of recycling and utilizing mulch are to directly oil or gasify the waste mulch through traditional pyrolysis devices. This treatment process has low oil and gas production, a wide variety of types, low selectivity, and low pyrolysis efficiency. In order to solve the above-mentioned problems of direct pyrolysis, a more advanced approach is to introduce catalysts such as zeolite and hydrocatalytic cracking during the pyrolysis process to accelerate the catalytic pyrolysis process. However, the small pore size of zeolite prevents the contact between the bulky polymer chains and the acid sites located in the pores of the zeolite, and the carbon deposition during the pyrolysis process will cause it to deactivate rapidly; the catalyst of hydrocatalytic cracking is difficult to control the sulfidation process of the metal and the uniform dispersion of the metal phase, and cannot ensure that the catalyst achieves the expected performance. Therefore, it is necessary to develop a membrane pyrolysis recovery catalyst based on existing technologies, which has low production cost, large pore size for easy loading, high catalytic efficiency, and easy recycling and reuse, and use it for the catalytic pyrolysis of polyethylene mulch, so as to provide a solution for the resource recycling of waste membranes for agricultural mulch and related industries using polyethylene membranes.

[0038] Kaolin is a stack of silicon-oxygen tetrahedron and aluminum-oxygen octahedron layered structures. As a catalyst carrier, it has the characteristics of abundant reserves, low price and high strength. It can increase the catalytic activity of the catalyst while increasing the material strength and pore size. Therefore, in order to solve the above technical problems, the inventors synergistically load trivalent iron ions and tungsten boric acid on kaolin with appropriate ratios and preparation processes to form a composite catalyst, and there is no need to go through the sulfidation process, which also fundamentally avoids the problem of uneven metal dispersion in the catalyst preparation process of hydrocatalytic cracking.

[0039] The drug-related information used in the embodiments of the present invention is as follows:

[0040] Sodium tungstate dihydrate (Na2WO4·2H2O, 98%), boric acid, glacial acetic acid, ferric nitrate, ferric chloride, ferric sulfate, ferric nitrate, ferric nitrate potassium chloride, and kaolin are all commercially available and prepared according to actual test needs. Among them, the average particle size of kaolin is 0.6-1.0 μm, and the Al2O3 content is ≥40%.

[0041] The stirring equipment, drying equipment, dripping equipment, water bath equipment, SEM and GC-MS instruments involved in the preparation method of the present invention are all commonly used equipment for experiments, as well as a pyrolysis reactor commonly used for pyrolysis of ground film.

[0042] The mulch used in the experiment was agricultural polyethylene mulch, which was uniformly collected and broken into small pieces for pyrolysis.

[0043] Embodiment 1

[0044] This embodiment provides a ferrotungstate / kaolin composite catalyst and its preparation and application method

[0045] 1. Raw materials and dosage

[0046] Sodium tungstate dihydrate (Na2WO4·2H2O, 98%): 1.0 kg;

[0047] Boric acid (10%): 0.2 kg;

[0048] Glacial acetic acid (5%): 0.1 g;

[0049] Ferric nitrate (10%): 1.2 kg;

[0050] Potassium chloride: 0.4kg;

[0051] Kaolin: 2.3kg;

[0052] Water: 25.7kg;

[0053] Ground film: 69.1kg.

[0054] 2. Process steps and parameters for preparing composite catalyst

[0055] (1) Synthesis of ferrotungstate K6[H2FeBW 11 O 40 ]·9H2O

[0056] 1.0 kg sodium tungstate dihydrate (Na2WO4·2H2O, 98%) and 0.2 kg boric acid (10%) were dissolved in 4.0 kg boiling water, and the pH value was adjusted to 6 with 0.1 kg 5% glacial acetic acid, and heated and stirred at 80°C for about 2 hours. The obtained mixed solution was placed in a 5°C environment for one day, and then filtered to remove the precipitate to obtain a reaction mixed solution. 1.2 kg 10% ferric nitrate solution was added dropwise to the reaction mixed solution, and the pH value was adjusted to 6 with 0.1 kg 5% glacial acetic acid again, and heated and stirred at 80°C for about 1 hour. After cooling to room temperature, 0.4 kg potassium chloride was added while stirring and mixed evenly, and the solid product was separated by filtration to obtain iron tungstate K6[H2FeBW 11 O 40 ]·9H2O solution.

[0057] (2) Preparation of ferrotungstate / kaolin composite catalyst

[0058] 2.3 kg of kaolin and 21.7 kg of water were mixed and stirred for 4 hours to uniformly disperse them to obtain a kaolin dispersion system. Then 2.3 kg of the iron tungstate solution prepared in the previous step was added dropwise to the kaolin dispersion system. The resulting mixture was stirred at 25°C (i.e., room temperature) for 12 hours and then heated in a 60°C water bath until most of the solvent evaporated. It was then dried in an oven at 105°C for 12 hours to obtain an iron tungstate / kaolin composite catalyst. The SEM image of the iron tungstate / kaolin composite catalyst was determined to be Figure 1 .

[0059] 3. Catalytic pyrolysis of ground film using ferrotungstate / kaolin composite catalyst

[0060] 69.1 kg of broken small pieces of mulch film and 2.5 kg of ferrotungstate / kaolin composite catalyst were uniformly mixed and placed in a pyrolysis reactor. After slowly heating to 350°C under a nitrogen flow, the nitrogen supply was stopped and the temperature of the pyrolysis reactor was kept unchanged until the catalytic pyrolysis reaction was completed, and finally 4.1 kg of coke and 53.8 kg of liquid oil were obtained, i.e., 77.8% of liquid oil and 16.2% of gas products.

[0061] The mass of the generated coke was determined by weighing the solid residue of the ground film raw material and the mass of the catalyst added before and after each test run. The yields of liquid oil and coke were calculated by dividing the mass of the obtained liquid oil and coke by the mass of the initial ground film raw material, i.e., liquid oil yield (%) = liquid oil mass / ground film raw material mass; coke yield (%) = coke mass / ground film raw material mass; the yield of the obtained gas product was: gas yield (%) = 1-liquid oil yield-coke yield.

[0062] Liquid oils obtained from non-catalytic and catalytic cracking of ground film were analyzed by gas chromatography / mass spectrometry. Each peak in the chromatogram belongs to a specific compound present in the oil sample. The mass spectrum of each compound was compared with the standard mass spectrum of the corresponding compound using the gas chromatography / mass spectrometry library (NIST / EPA / NIH mass spectrometry library). We selected about 35 major peaks and quantified them. The similarity index for compound identification was maintained at >90. Table 2 provides the identification of the relative abundance of all compounds. It can be seen that the main components of the liquid oil are paraffins and olefins (C5-C26). A wide range of hydrocarbons (C6-C26) are present in the liquid oil produced by cracking of ground film without the use of a catalyst. We found that most of the liquid oil is composed of higher molecular weight hydrocarbons. The liquid oil produced by catalytic cracking of ground film using a ferrotungstate / kaolin composite catalyst showed a large amount of lighter hydrocarbons, especially in the gasoline range (C5-C 12 ) hydrocarbons. The gaseous products are organic gases with lower C numbers.

[0063] Embodiment 2

[0064] This embodiment provides a ferrotungstate / kaolin composite catalyst for catalytic cracking of ground film and its preparation and application method

[0065] 1. Raw materials and dosage

[0066] Sodium tungstate dihydrate (Na2WO4·2H2O, 98%): 1.0 kg;

[0067] Boric acid (10%): 0.2 kg;

[0068] Glacial acetic acid (5%): 0.1 g;

[0069] Ferric chloride (20%): 1.2 kg;

[0070] Potassium chloride: 0.4kg;

[0071] Kaolin: 2.3kg;

[0072] Water: 25.7kg;

[0073] Ground film: 69.1kg.

[0074] 2. Process steps and parameters for preparing composite catalyst

[0075] (1) Synthesis of ferrotungstate K6[H2FeBW 11 O 40 ]·9H2O

[0076] The method is the same as that in Example 1, except that 1.2 kg of 20% ferric chloride solution is added dropwise to the reaction mixture of sodium tungstate-boric acid-water, the pH value is adjusted to 6 again, and the mixture is heated and stirred at 80°C for about 1 hour. After cooling to room temperature, 0.4 kg of potassium chloride is added while stirring and mixed evenly, and the solid product is separated by filtration to obtain ferrotungstate K6[H2FeBW 11 O 40 ]·9H2O.

[0077] (2) Preparation of ferrotungstate / kaolin composite catalyst

[0078] The operation is the same as that of the first embodiment.

[0079] (3) Catalytic pyrolysis of ground film using ferrotungstate / kaolin composite catalyst

[0080] The method is the same as that of Example 1, except that 3.5 kg of coke and 54.7 kg of liquid oil are finally obtained, namely 79.1% of liquid oil and 15.8% of gas products.

[0081] Embodiment 3

[0082] This embodiment provides a ferrotungstate / kaolin composite catalyst for catalytic cracking of ground film and its preparation and application method

[0083] 1. Raw materials and dosage

[0084] Sodium tungstate: 1.0kg;

[0085] Boric acid (10%): 0.2 kg;

[0086] Glacial acetic acid (5%): 0.1 g;

[0087] Ferrous sulfate (30%): 1.2 kg;

[0088] Potassium chloride: 0.4kg;

[0089] Kaolin: 2.3kg;

[0090] Water: 25.7kg;

[0091] Ground film: 69.1kg.

[0092] 2. Process steps and parameters

[0093] (1) Synthesis of ferrotungstate K6[H2FeBW 11 O 40 ]·9H2O

[0094] The steps for synthesizing tungstate iron are the same as those in Example 1, except that 1.2 kg of 30% by mass ferric sulfate solution is added dropwise to the reaction mixture of sodium tungstate-boric acid-water, the pH value is adjusted to 6 again, and the mixture is heated and stirred at 80°C for about 1 hour. After cooling to room temperature, 0.4 kg of potassium chloride is added while stirring and mixed evenly, and the solid product is separated by filtration to obtain tungstate iron K6[H2FeBW 11 O 40 ]·9H2O.

[0095] (2) Preparation of ferrotungstate / kaolin composite catalyst

[0096] The same operation steps are used as in Example 1. The SEM image of the ferrotungstate / kaolin composite catalyst can be found in Figure 2 .

[0097] (3) Catalytic pyrolysis of ground film using ferrotungstate / kaolin composite catalyst

[0098] The method is the same as that of Example 1, except that 2.4 kg of coke and 55.9 kg of liquid oil are finally obtained in this example, that is, 81.0% of liquid oil and 15.5% of gas products.

[0099] Embodiment 4

[0100] This embodiment provides a ferrotungstate / kaolin composite catalyst for catalytic cracking of ground film and its preparation and application method

[0101] 1. Raw materials and dosage

[0102] Sodium tungstate: 1.0kg;

[0103] Boric acid (10%): 0.2 kg;

[0104] Glacial acetic acid (5%): 0.1 g;

[0105] Ferric nitrate (40%): 1.2 kg;

[0106] Potassium chloride: 0.4kg;

[0107] Kaolin: 2.3kg;

[0108] Water: 25.7kg;

[0109] Ground film: 69.1kg.

[0110] 2. Process steps and parameters for preparing composite catalyst

[0111] (1) Synthesis of ferrotungstate K6[H2FeBW 11 O 40 ]·9H2O

[0112] The method is the same as that in Example 1, except that 1.2 kg of 40% iron nitrate solution is added dropwise to the filtrate obtained by filtration, the pH value is adjusted to 6 again, and the mixture is heated and stirred at 80°C for about 1 hour. After cooling to room temperature, 0.4 kg of potassium chloride is added while stirring and mixed evenly, and the solid product is separated by filtration to obtain iron tungstate K6[H2FeBW 11 O 40 ]·9H2O.

[0113] (2) Preparation of ferrotungstate / kaolin composite catalyst

[0114] The operation is the same as that of the first embodiment.

[0115] (3) Catalytic pyrolysis of ground film using ferrotungstate / kaolin composite catalyst

[0116] The method is the same as that of Example 1, except that 2.3 kg of coke and 56.7 kg of liquid oil are finally obtained, namely 82.1% of liquid oil and 14.5% of gas products.

[0117] Embodiment 5

[0118] This embodiment provides a ferrotungstate / kaolin composite catalyst for catalytic cracking of ground film and its preparation and application method

[0119] 1. Raw materials and dosage

[0120] Sodium tungstate: 1.0kg;

[0121] Boric acid (10%): 0.2 kg;

[0122] Glacial acetic acid (5%): 0.1 g;

[0123] Ferric nitrate (50%): 1.2 kg;

[0124] Potassium chloride: 0.4kg;

[0125] Kaolin: 2.3kg;

[0126] Water: 25.7kg.

[0127] Ground film: 69.1kg.

[0128] 2. Process steps and parameters for preparing composite catalyst

[0129] (1) Synthesis of ferrotungstate K6[H2FeBW 11 O 40]·9H2O

[0130] 1.0 kg sodium tungstate dihydrate (Na2WO4·2H2O, 98%) and 0.2 kg boric acid (10%) were dissolved in 4.0 kg boiling water, and the pH value was adjusted to 7 with 0.1 kg 5% glacial acetic acid, and heated and stirred at 80°C for about 2 hours. The obtained mixed solution was placed in a 5°C environment for one day, and then filtered to remove the precipitate to obtain a reaction mixed solution. 1.2 kg 10% ferric nitrate solution was added dropwise to the reaction mixed solution, and the pH value was adjusted to 7 again, and heated and stirred at 80°C for about 1 hour. After cooling to room temperature, 0.4 kg potassium chloride was added thereto while stirring and mixed evenly, and the solid product was separated by filtration to obtain iron tungstate K6[H2FeBW 11 O 40 ]·9H2O.

[0131] (2) Preparation of ferrotungstate / kaolin composite catalyst

[0132] The operation is the same as in Example 1. The SEM image of the ferrotungstate / kaolin composite catalyst is shown in Figure 3 .

[0133] (3) Catalytic pyrolysis of ground film using ferrotungstate / kaolin composite catalyst

[0134] The method is the same as that of Example 1, except that 2.1 kg of coke and 57.3 kg of liquid oil are finally obtained, namely 82.9% of liquid oil and 14.1% of gas products.

[0135] Embodiment 6

[0136] This embodiment provides a ferrotungstate / kaolin composite catalyst and its preparation and application method

[0137] 1. Raw materials and dosage

[0138] Sodium tungstate: 1.7kg;

[0139] Boric acid (10%): 0.2 kg;

[0140] Glacial acetic acid (5%): 0.1 g;

[0141] Ferric nitrate (10%): 1.4 kg;

[0142] Potassium chloride: 0.4kg;

[0143] Kaolin: 3.5kg;

[0144] Water: 26.7kg;

[0145] Ground film: 60.0kg.

[0146] 2. Process steps and parameters for preparing composite catalyst

[0147] (1) Synthesis of ferrotungstate K6[H2FeBW 11 O 40 ]·9H2O

[0148] 1.7 kg sodium tungstate dihydrate (Na2WO4·2H2O, 98%) and 0.2 kg boric acid (10%) were dissolved in 3.4 kg boiling water, and the pH value was adjusted to 6 with 0.1 kg 5% glacial acetic acid, and heated and stirred at 80°C for about 2 hours. The obtained mixed solution was placed in a 5°C environment for one day, and then filtered to remove the precipitate to obtain a reaction mixed solution. 1.4 kg 10% ferric nitrate solution was added dropwise to the reaction mixed solution, and the pH value was adjusted to 6 again, and heated and stirred at 80°C for about 1 hour. After cooling to room temperature, 0.4 kg potassium chloride was added while stirring and mixed evenly, and the solid product was separated by filtration to obtain iron tungstate K6[H2FeBW 11 O 40 ]·9H2O.

[0149] (2) Preparation of ferrotungstate / kaolin composite catalyst

[0150] 3.5 kg of kaolin and 23.3 kg of water were mixed and stirred for 4 hours to uniformly disperse them to obtain a kaolin dispersion system. Then 3.3 kg of the ferrotungstate solution prepared in the previous step was dropwise added to the kaolin dispersion system. The resulting mixture was stirred at 25°C (i.e., room temperature) for 12 hours and then heated in a 60°C water bath until most of the solvent evaporated, and then dried in an oven at 105°C for 12 hours to obtain a ferrotungstate / kaolin composite catalyst.

[0151] 3. Catalytic pyrolysis of ground film using ferrotungstate / kaolin composite catalyst

[0152] 60.0 kg of broken small pieces of mulch film and 6.0 kg of tungstate iron / kaolin composite catalyst were uniformly mixed and placed in a pyrolysis reactor. After slowly heating to 350°C under a nitrogen flow, the nitrogen supply was stopped and the temperature of the pyrolysis reactor was kept unchanged until the catalytic pyrolysis reaction was completed, and finally 3.7 kg of coke and 47.2 kg of liquid oil were obtained, i.e., 78.6% of liquid oil and 15.3% of gas products.

[0153] Embodiment 7

[0154] This embodiment provides a ferrotungstate / kaolin composite catalyst and its preparation and application method

[0155] 1. Raw materials and dosage

[0156] Sodium tungstate: 1.0kg;

[0157] Boric acid (10%): 0.2 kg;

[0158] Glacial acetic acid (5%): 0.1 g;

[0159] Ferric nitrate (10%): 1.2 kg;

[0160] Potassium chloride: 0.4kg;

[0161] Kaolin: 2.3kg;

[0162] Water: 25.7kg;

[0163] Ground film: 69.1kg.

[0164] 2. Process steps and parameters for preparing composite catalyst

[0165] (1) Synthesis of ferrotungstate K6[H2FeBW 11 O 40 ]·9H2O

[0166] The operation is the same as that of the first embodiment.

[0167] (2) Preparation of ferrotungstate / kaolin composite catalyst

[0168] The operation is the same as that of the first embodiment.

[0169] (3) Catalytic pyrolysis of ground film using ferrotungstate / kaolin composite catalyst

[0170] The method is the same as that of Example 1, except that the reaction temperature is 400° C., and finally 4.2 kg of coke and 53.9 kg of liquid oil are obtained, that is, 78.0% of liquid oil and 15.9% of gas products.

[0171] Comparative Example 1

[0172] Direct pyrolysis of ground film without adding catalyst

[0173] 100 kg of ground film was placed in a pyrolysis reactor consistent with Examples 1 to 7, and slowly heated to 400°C under a nitrogen flow. The nitrogen supply was stopped and the temperature of the reactor was kept unchanged until the catalytic pyrolysis reaction was completed, and finally 23.0 kg of coke and 67.9 kg of liquid oil were obtained, i.e., 67.9% of liquid oil and 9.1% of gas products.

[0174] Comparative Example 2

[0175] 1. Recycling of ferrotungstate / kaolin composite catalyst

[0176] The ferrotungstate / kaolin composite catalyst used in Example 5 was washed with ethanol and dried in an oven at 105° C. for 12 h to obtain a recovered ferrotungstate / kaolin composite catalyst II.

[0177] 2. Use the recycled iron tungstate / kaolin composite catalyst to catalyze the pyrolysis of ground film

[0178] 96 kg of ground film and 4 kg of recycled tungstate iron / kaolin composite catalyst II were uniformly mixed and placed in a pyrolysis reactor. After slowly heating to 350°C under a nitrogen flow, the nitrogen supply was stopped and the temperature of the reactor was kept unchanged until the catalytic pyrolysis reaction was completed, and finally 3.2 kg of coke and 79.0 kg of liquid oil were obtained, i.e., 82.3% of liquid oil and 14.4% of gas products.

[0179] The process parameters and yields of various products involved in the catalytic pyrolysis method of the film used in the above-mentioned Examples 1 to 7, Comparative Examples 1 and 2 are detailed in Table 1.

[0180] Table 1 Process parameters and liquid oil and gas yields of Examples 1 to 7 of the present invention and Comparative Examples 1 and 2

[0181]

[0182]

[0183] The identification of various hydrocarbons produced by catalytic pyrolysis of mulch films using different catalysts in the above-mentioned Examples 1 to 7, Comparative Examples 1 and 2 is shown in Table 2.

[0184] Table 2 Identification of various hydrocarbon compounds in Examples 1 to 7 of the present invention, Comparative Example 1 and Comparative Example 2

[0185]

[0186]

[0187] From the contents shown in Table 1, it can be seen that by comparing Examples 1 to 5 with Comparative Example 1, it is found that under the action of 10%, 20%, 30%, 40% and 50% by mass fraction of ferrotungstate / kaolin composite catalyst, the pyrolysis temperature of the mulch film is reduced from 400°C to 350°C, and the pyrolysis time is reduced from 3h to 2h, 1.30h, 1h, 1h and 1h, respectively. Compared with the case where no ferrotungstate / kaolin composite catalyst is used, the catalytic pyrolysis conversion rate of the mulch film is significantly improved, and the liquid oil yield is increased by 14.6%, 16.5%, 19.3%, 20.9% and 22.1%, respectively, and the gas yield is increased by 78.0%, 73.6%, 70.3%, 59.3% and 53.8%, respectively. Comparing Example 2 with Example 1, it was found that after the mass fraction of the iron tungstate / kaolin composite catalyst used was increased from 10% to 20%, the pyrolysis time was shortened by 30min, the liquid oil yield was increased by 1.7%, and the gas yield was slightly decreased. Comparing Example 3 with Example 2, it was found that after the mass fraction of the iron tungstate / kaolin composite catalyst used was increased from 20% to 30%, the pyrolysis time was shortened by 30min when the pyrolysis temperature was 350°C, and the liquid oil yield was slightly increased. Comparing Example 5, Example 4 and Example 3, it was found that after the mass fraction of the iron tungstate / kaolin composite catalyst used was increased from 30% to 40% and 50%, the pyrolysis time of the ground film remained unchanged, and the liquid oil yield was gradually slightly increased. Comparing Example 6 with Example 1, it was found that after the amount of the iron tungstate / kaolin composite catalyst used was increased to one-tenth of the mass of the ground film, the pyrolysis time was shortened by 1h, and the liquid oil yield and gas yield were not much different. Comparing Example 7 with Example 1, it is found that after the pyrolysis temperature of the ground film is increased to 400°C, the pyrolysis time is shortened by 30 minutes, and the liquid oil yield and gas yield are slightly improved. Comparing Example 5 with Comparative Example 2, it is found that after the used 50% mass fraction of iron tungstate / kaolin composite catalyst is recycled and reused, the pyrolysis temperature and pyrolysis time of the ground film remain unchanged, and the liquid oil yield and gas yield are not much different, indicating that the iron tungstate / kaolin composite catalyst maintains its original good catalytic performance after recycling. It can be seen that when only the iron tungstate / kaolin composite catalyst with a mass fraction of 30% is used, the pyrolysis time can be shortened to 1 hour when the pyrolysis temperature is 350°C, and the liquid oil yield and gas yield are as high as 81.0% and 15.5%. On the one hand, the catalytic pyrolysis temperature and pyrolysis time were reduced, that is, the ideal liquid oil yield and gas yield can be achieved by treating at 350°C for only 1 hour, which greatly saves the energy consumption required for the catalytic pyrolysis process; on the other hand, the amount of ferrotungstate / kaolin composite catalyst used in the catalytic pyrolysis process was reduced, which greatly reduced the consumption of resources, and the yield of liquid oil and gas products converted from catalytic pyrolysis of the film was greatly improved.In summary, after introducing the iron tungstate / kaolin composite catalyst, the yield of catalytic cracking of mulch into liquid oil and gas products is significantly improved while reducing the pyrolysis temperature and pyrolysis time. Preferably, when using a 30% by mass iron tungstate / kaolin composite catalyst, the pyrolysis temperature is 350°C, the pyrolysis time is 1h, and the liquid oil yield and gas yield are as high as 81.0% and 15.5%, respectively. While saving resources and energy, the catalytic pyrolysis conversion efficiency of mulch is improved, thereby realizing the resource utilization of recycled waste mulch.

[0188] The catalytic pyrolysis treatment of ground film by using the iron tungstate / kaolin composite catalyst provided by the present invention can solve the technical problems of low oil and gas yield in the traditional catalytic pyrolysis process and high cost of existing catalysts when recycling waste ground film, and realize its resource utilization. Since the iron tungstate / kaolin composite catalyst is used, the catalytic pyrolysis performance is improved by loading iron tungstate on kaolin to produce additional Lewis acid sites and Bronsted acid sites, the pyrolysis temperature and pyrolysis time of the ground film are reduced, and the energy required in the pyrolysis process is greatly reduced. At the same time, by shortening the reaction time, the secondary reaction is prevented from producing aromatic compounds, and the yield of light hydrocarbons after catalytic pyrolysis of the ground film is improved. The product has a high content of fuel oil in the range of C5-C12. The use of relatively low-priced kaolin as a catalyst raw material saves the cost of the ground film cracking resource utilization process, and has good economic and environmental benefits. Due to the good properties of kaolin, the ferrotungstate / kaolin composite catalyst has good thermal stability, is easy to recycle, and can be recycled multiple times compared with traditional catalysts. It solves the defects of traditional catalysts that are difficult to recycle or the catalytic performance is greatly reduced after recycling. It is expected to be applied to large-scale catalytic pyrolysis processes in the mulch film industry.

[0189] It should be noted that, although the above embodiments have been described in this article, the patent protection scope of the present invention is not limited thereby. Therefore, based on the innovative concept of the present invention, changes and modifications made to the embodiments described herein, or equivalent structures or equivalent process changes made using the contents of the present invention specification and drawings, directly or indirectly applying the above technical solutions to other related technical fields, are all included in the patent protection scope of the present invention.

Claims

1. A method for preparing a composite catalyst, It is characterized in that The following steps are involved: Tungstate, water and boric acid are mixed in a mass ratio of 5 to 10:20:1, reacted at a certain pH value and a certain temperature to obtain a reaction mixture system, allowed to stand, and the precipitate is removed to obtain a reaction mixture solution; The trivalent iron salt solution is added dropwise to the reaction mixture solution, reacted at a certain pH value and a certain temperature, cooled to room temperature, and potassium salt is added and mixed evenly, wherein the mass ratio of potassium salt to boric acid is 2 to 3:1, and the solid matter is separated and removed, and washed to obtain iron tungstate K 6 [H 2 FWf 11 O 40 ]·9H 2 O; The obtained reaction mixture system and the obtained ferrotungstate K 6 [H 2 FWf 11 O 40 ]·9H 2 The reaction pH value of step O is 6-7, and the reaction temperature is 80℃-90℃; Kaolin and water are uniformly mixed in a mass ratio of 1 to 3:20, and a 10% to 50% by mass iron tungstate solution is added dropwise, and the mixture is placed in a water bath for reaction to obtain the composite catalyst.

2. The preparation method according to claim 1, It is characterized in that The temperature of the reaction mixture system after standing is 0°C to 10°C, the standing time is 12h to 36h, and the temperature of the water bath is 60°C to 80°C.

3. A composite catalyst prepared by the preparation method according to claim 1 or 2.

4. A method for catalytically pyrolyzing ground film using the composite catalyst according to claim 3, It is characterized in that The following steps are involved: The composite catalyst and the ground film are mixed at a mass ratio of 10 to 27.6:1, placed in a pyrolysis reactor, and heated for a certain period of time in an inert gas environment.

5. The method according to claim 4, It is characterized in that The heating reaction temperature is 350°C to 400°C.