A near-infrared-magnetic response shape memory photocurable ink and its preparation method and application

By preparing near-infrared-magnetic response shape memory light curing ink, the problem of inappropriate glass transition temperature of polyurethane materials and low dispersion of Fe3O4 magnetic nanoparticles was solved, and the near-infrared-magnetic response capability and mechanical properties of the material were improved, and successfully The printing of vascular branch stents in digital light processing 3D printing technology has expanded its application range in the field of medicine.

CN116715990BActive Publication Date: 2024-11-12LANZHOU INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES +2
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310679204.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-09
Publication Date
2024-11-12
Estimated Expiration
2043-06-09

AI Technical Summary

Technical Problem

In the field of biomedical science, the existing polyurethane materials are not suitable for glass transition temperature and are difficult to achieve complex deformation, and the low dispersion of Fe3O4 magnetic nanoparticles in the matrix, which limits their application in complex medical environments, especially in digital light processing. There are very few applications in 3D printing technology.

Method used

By adding polytetrahydrofuran and diisocyanate, a prepolymer is obtained and polymerized with the first acrylate, dopamined Fe3O4 magnetic nanoparticles, polymerization inhibitors and photoinitiators are added to prepare a near-infrared-magnetic response shape Memory light curing ink improves the dispersion and mechanical properties of the material, reduces the glass transition temperature, and makes it suitable for the human body temperature range.

Benefits of technology

It realizes the near-infrared-magnetic response capability of the material, reduces the glass transition temperature to the physiological temperature range, improves the mechanical properties, and is successfully applied to the printing of vascular branch stents in digital light processing 3D printing technology, with a wide range of medical application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116715990B_ABST
    Figure CN116715990B_ABST
Patent Text Reader

Abstract

The present invention provides a near-infrared magnetic response shape memory photocurable ink and a preparation method and application thereof, belonging to the technical field of polymer materials. The present invention provides a method for preparing a near-infrared magnetic response shape memory photocurable ink, comprising the following steps: mixing polytetrahydrofuran and diisocyanate for addition reaction to obtain a prepolymer; mixing the prepolymer and a first acrylate for polymerization reaction to obtain a polyurethane prepolymer; mixing the polyurethane prepolymer, the second acrylate, and dopamine Fe 3 O 4 The magnetic nanoparticles, the polymerization inhibitor and the photoinitiator are mixed to obtain the near-infrared-magnetic responsive shape memory photocurable ink. The shape memory polymer prepared by the present invention not only has a suitable glass transition temperature and mechanical properties, but also has excellent near-infrared-magnetic responsiveness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of polymer materials, and in particular to a near-infrared-magnetic response shape memory photocurable ink and a preparation method and application thereof. Background Art

[0002] Polyurethane (PU) materials have excellent fatigue resistance, wear resistance, high elasticity and high strength. The microphase separation structure makes it have better biocompatibility (including blood compatibility and tissue compatibility) than other polymer materials. It is widely used in the field of biomedical materials. The cross-linked PU also has shape memory function, but its glass transition temperature is too high or too low to be suitable for the human body; shape memory polymers have a single stimulus response and are difficult to perform complex deformations, which limits their multiple deformations in complex medical environments. Magnetic response and near-infrared response can realize non-contact triggering of materials, which is suitable for operations in narrow or confined spaces of the human body, but shape memory materials with both are rarely reported. Fe3O4 magnetic nanoparticles have good biocompatibility and biodegradability, and have good magnetic field response capabilities, but the nanoparticles are prone to agglomeration in the matrix, resulting in low dispersibility.

[0003] Digital light processing 3D printing technology (DLP) is a new printing technology with fast printing efficiency, high precision, low energy consumption and high product strength. It is an ideal printing method in the biomedical field, but it has high requirements for printing ink. Currently, there are very few reports on the application of Fe3O4 magnetic nanoparticles in DLP printing. Summary of the invention

[0004] In view of this, the object of the present invention is to provide a near-infrared-magnetic responsive shape memory photocurable ink and its preparation method and application. The shape memory polymer prepared by the photocurable ink of the present invention not only has a suitable glass transition temperature and mechanical properties, but also has excellent near-infrared-magnetic responsiveness.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a near-infrared-magnetic response shape memory photocurable ink, comprising the following steps:

[0007] The polytetrahydrofuran and diisocyanate are mixed and subjected to addition reaction to obtain a prepolymer;

[0008] The prepolymer and the first acrylate are mixed to carry out polymerization reaction to obtain a polyurethane prepolymer;

[0009] The polyurethane prepolymer, the second acrylate, dopaminated Fe3O4 magnetic nanoparticles, an inhibitor and a photoinitiator are mixed to obtain the near-infrared-magnetic responsive shape memory photocurable ink.

[0010] Preferably, the first acrylate and the second acrylate independently include one or more of hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, methyl 2-methacrylate and ethyl 2-methacrylate.

[0011] Preferably, the mass ratio of the polyurethane prepolymer, the second acrylate, the dopaminated Fe3O4 magnetic nanoparticles, the inhibitor and the photoinitiator is 9:12-30:0.9:0.03:0.3-0.6.

[0012] Preferably, the dopaminated Fe3O4 magnetic nanoparticles have Fe3O4 magnetic nanoparticles as cores and polydopamine as shells, the mass ratio of the Fe3O4 magnetic nanoparticles to polydopamine is 0.8-1.6:1, and the particle size of the Fe3O4 magnetic nanoparticles is 50 nm.

[0013] Preferably, the mass ratio of the polytetrahydrofuran to diisocyanate is 40:6.72.

[0014] Preferably, the mass ratio of the polytetrahydrofuran to the first acrylate is 40:5.2.

[0015] Preferably, the diisocyanate includes naphthalene diisocyanate, 4,4-diphenylmethane diisocyanate, toluene diisocyanate or hexamethylene diisocyanate.

[0016] The present invention also provides near-infrared-magnetic response shape memory photocurable ink prepared by the preparation method described in the above technical solution.

[0017] The present invention also provides the use of the near-infrared-magnetic response shape memory photocurable ink described in the above technical solution in the preparation of shape memory polymers.

[0018] The present invention also provides the use of the near-infrared-magnetic response shape memory photocurable ink described in the above technical solution in the preparation of a blood vessel branch stent.

[0019] The invention provides a method for preparing near-infrared-magnetic response shape memory photocurable ink, comprising the following steps: mixing polytetrahydrofuran and diisocyanate for addition reaction to obtain a prepolymer; mixing the prepolymer and a first acrylate for polymerization reaction to obtain a polyurethane prepolymer; and mixing the polyurethane prepolymer, a second acrylate, dopaminated Fe3O4 magnetic nanoparticles, an inhibitor and a photoinitiator to obtain the near-infrared-magnetic response shape memory photocurable ink.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] In the present invention, the dopamine-modified Fe3O4 magnetic nanoparticles effectively overcome the agglomeration phenomenon of the Fe3O4 magnetic nanoparticles, improve their dispersibility in PU, and dopamine gives the material excellent near-infrared response ability. More importantly, by adding dopamine-modified Fe3O4 magnetic nanoparticles to PU, the transition temperature of the material is reduced to within the physiological temperature range (37.7°C). The reason is that the surface of the dopamine-modified Fe3O4 magnetic nanoparticles is rich in -NH2 and -OH2, which form a regular structure by forming hydrogen bonds with the long chains of polyurethane, thereby making the soft segments and hard segments inside the polyurethane The hydrogen bonds between the hard segments are dissociated, which reduces the restriction of the hard segments on the soft segments, the soft phase is separated, the restriction of the hard segments on the polyurethane chains is reduced, and the polyurethane chains are easier to move, so the glass transition temperature is reduced. In addition, due to the rigidity of the Fe3O4 nanoparticles and the introduction of hydrogen bonds, the mechanical strength of the material is increased, and the mechanical properties are improved. The acrylate of the present invention is used as a prepolymer dispersant and a raw material for photocuring reaction. The "solvent-free" polymerization mode improves the mechanical properties of the material. The acrylate double bond group enables the material to have ultraviolet light curing ability. By adding a photoinitiator and an inhibitor to form a polyurethane photosensitive ink, it is successfully applied to digital light processing 3D printing technology (DLP) and can perform fine printing.

[0022] The present invention also provides a near-infrared-magnetic responsive shape memory photocurable ink prepared by the preparation method described in the above technical scheme. The shape memory polymer prepared using the near-infrared-magnetic responsive shape memory photocurable ink prepared by the present invention not only has a suitable glass transition temperature and mechanical properties, but also has excellent near-infrared-magnetic response ability. The DLP printing technology is successfully used to print vascular branch stents, which is expected to be used in the research and development of medical intracavitary grafts (stents, venous filters, occluders, etc.), and to help develop personalized precision medicine. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Transmission electron microscopy images of agglomerated Fe3O4 magnetic nanoparticles without dopamine modification (left) and dopamine-modified Fe3O4 magnetic nanoparticles (right);

[0024] Figure 2 A differential scanning calorimetry analysis curve of the ink photocured film in Comparative Example 1;

[0025] Figure 3 The differential scanning calorimetry analysis curve of the ink photocured film in Example 3;

[0026] Figure 4 A is a real picture of the DLP printer, B is a branched vascular stent model designed by Blender software, and C is a real picture of the multi-responsive branched vascular stent printed by DLP;

[0027] Figure 5 A and D are the magnetic response capabilities of the shape memory polymer material obtained in Example 3, B is the near-infrared response capability, and C is the infrared imager image of the stent after the test. DETAILED DESCRIPTION

[0028] The present invention provides a method for preparing a near-infrared-magnetic response shape memory photocurable ink, comprising the following steps:

[0029] The polytetrahydrofuran and diisocyanate are mixed and subjected to addition reaction to obtain a prepolymer;

[0030] The prepolymer and the first acrylate are mixed to carry out polymerization reaction to obtain a polyurethane prepolymer;

[0031] The polyurethane prepolymer, the second acrylate, dopaminated Fe3O4 magnetic nanoparticles, an inhibitor and a photoinitiator are mixed to obtain the near-infrared-magnetic responsive shape memory photocurable ink.

[0032] In the present invention, unless otherwise specified, the raw materials used are all commercially available products in the art.

[0033] The invention mixes polytetrahydrofuran (PTMEG) and diisocyanate to carry out addition reaction to obtain a prepolymer.

[0034] In the present invention, the number average molecular weight of the polytetrahydrofuran is preferably 250-3000, more preferably 2000.

[0035] In the present invention, the diisocyanate preferably includes naphthalene diisocyanate, 4,4-diphenylmethane diisocyanate, toluene diisocyanate or hexamethylene diisocyanate (HDI).

[0036] In the present invention, the mass ratio of the polytetrahydrofuran to the diisocyanate is preferably 40:6.72.

[0037] In the present invention, the polytetrahydrofuran is preferably dried before use, and the drying is preferably carried out by placing it in a vacuum oven at 80° C. for 8 hours.

[0038] In the present invention, the temperature of the addition reaction is preferably 80-85° C., the time is preferably 2-3 hours, and the addition reaction is preferably carried out in a nitrogen atmosphere.

[0039] In the present invention, the polytetrahydrofuran and diisocyanate are preferably poured into a three-necked flask to be fully dissolved, the temperature is raised to the temperature of the addition reaction, condensed and refluxed under a nitrogen atmosphere, and mechanically stirred to carry out the addition reaction.

[0040] After obtaining the prepolymer, the present invention mixes the prepolymer and the first acrylate to carry out polymerization reaction to obtain a polyurethane prepolymer.

[0041] In the present invention, the first acrylate preferably includes one or more of hydroxyethyl methacrylate (HEMA), dimethylaminoethyl methacrylate (DMAEMA), 2-methyl methacrylate and 2-ethyl methacrylate, and more preferably includes hydroxyethyl methacrylate and dimethylaminoethyl methacrylate. The mass ratio of hydroxyethyl methacrylate to dimethylaminoethyl methacrylate is preferably 2:5, 1:1 or 5:2.

[0042] In the present invention, the first acrylate is preferably used after purification treatment, and the purification treatment preferably includes the following steps: filtering the acrylate through an alkaline alumina solid phase extraction column to remove residual inhibitor and moisture, and sealing and refrigerating for standby use.

[0043] In the present invention, the mass ratio of the polytetrahydrofuran to the first acrylate is preferably 40:5.2.

[0044] In the present invention, the polymerization reaction temperature is preferably 80-85° C., the time is preferably 2-3 hours, and the polymerization reaction is preferably carried out in a nitrogen atmosphere.

[0045] In the present invention, the first acrylate is preferably preheated to the polymerization reaction temperature and then added to the prepolymer, and the polymerization reaction is carried out under a nitrogen atmosphere with mechanical stirring.

[0046] After the polymerization reaction is completed, the present invention preferably pours the reacted sample into a glass reagent bottle while it is hot, puts it into a 60° C. vacuum oven to remove bubbles, and cools it to room temperature to obtain the polyurethane prepolymer, which has an appearance of a white waxy solid and is preferably sealed and stored at room temperature.

[0047] Taking hexamethylene diisocyanate and hydroxyethyl methacrylate as examples, the principle of preparing the polyurethane prepolymer is shown in the following formula:

[0048]

[0049] After obtaining the polyurethane prepolymer, the present invention mixes the polyurethane prepolymer, the second acrylate, dopaminated Fe3O4 magnetic nanoparticles, an inhibitor and a photoinitiator to obtain the near-infrared-magnetic responsive shape memory photocurable ink.

[0050] In the present invention, the second acrylate preferably includes one or more of hydroxyethyl methacrylate (HEMA), dimethylaminoethyl methacrylate (DMAEMA), 2-methyl methacrylate and 2-ethyl methacrylate, and more preferably includes hydroxyethyl methacrylate and dimethylaminoethyl methacrylate. The mass ratio of hydroxyethyl methacrylate to dimethylaminoethyl methacrylate is preferably 2:5, 1:1 or 5:2.

[0051] In the present invention, the mass ratio of the polyurethane prepolymer, the second acrylate, the dopaminated Fe3O4 magnetic nanoparticles, the inhibitor and the photoinitiator is preferably 9:12-30:0.9:0.03:0.3-0.6, and more preferably 9:15-21:0.9:0.03:0.3-0.6.

[0052] In the present invention, the dopaminated Fe3O4 magnetic nanoparticles preferably have Fe3O4 magnetic nanoparticles as cores and polydopamine as shells, the mass ratio of the Fe3O4 magnetic nanoparticles to polydopamine is preferably 0.8-1.6:1, and the particle size of the Fe3O4 magnetic nanoparticles is preferably 50 nm.

[0053] In a specific embodiment of the present invention, the method for preparing the dopaminated Fe3O4 magnetic nanoparticles preferably comprises the following steps:

[0054] Weigh tris(hydroxymethyl)aminomethane) into a 500 mL round-bottom flask, pour in ultrapure water, adjust the pH value of the solution to 8.5 with hydrochloric acid, add Fe3O4 magnetic nanoparticles into the flask, and disperse them evenly in the solution by high-frequency ultrasound for 4 hours. The resulting solution is black, add dopamine hydrochloride powder to the solution, mechanically stir for 24 hours at room temperature, pour the mixed solution into a beaker, then let it stand for 30 minutes, and place a strong magnet underneath to accelerate the sedimentation of the Fe3O4 magnetic nanoparticles, pour out the brown-black upper liquid, and wash the resulting lower black precipitate with ultrapure water and anhydrous ethanol for several times until the washing liquid becomes light yellow and neutral. Finally, the resulting black precipitate is placed in a vacuum oven at 40°C for 48 hours to obtain the dopaminized Fe3O4 magnetic nanoparticles.

[0055] In the present invention, the inhibitor preferably includes one or more of hydroquinone, 2,6-di-tert-butyl-p-cresol, 2,5-di-tert-butyl-hydroquinone and 2-tert-butyl-hydroquinone. The function of the inhibitor is to slow down the self-polymerization of the ink before 3D printing and improve the printing performance.

[0056] In the present invention, the photoinitiator preferably includes one or more of dimethyl benzil ether (DMPA), (2,4,6-trimethylbenzamido)diphenylphosphine oxide (TPO), (2,4,6-trimethylbenzamido)ethyl phosphonate, 2-hydroxy-2-methyl-1-phenylpropanone, 2,4-diethylthioxanthone and benzophenone.

[0057] In the present invention, the mixing preferably includes the following steps: placing the second acrylate in a round-bottom flask, adding the dopaminated Fe3O4 magnetic nanoparticles, high-frequency ultrasound for 2 hours, adding the polyurethane prepolymer to the mixed solution, mechanically stirring for 1 hour at 40°C in a N2 atmosphere to obtain a dark black solution, and finally adding the inhibitor and photoinitiator, and continuing to stir for 0.5 hours at 40°C while wrapped in tin foil to avoid light.

[0058] The present invention also provides near-infrared-magnetic response shape memory photocurable ink prepared by the preparation method described in the above technical solution.

[0059] The present invention also provides the use of the near-infrared-magnetic response shape memory photocurable ink described in the above technical solution in the preparation of shape memory polymers.

[0060] The present invention preferably pours the mixed near-infrared-magnetic responsive shape memory photocurable ink into a preheated polytetrafluoroethylene mold, degassing it in a 40° C. vacuum oven for 10 minutes, and then photocuring it to obtain the shape memory polymer.

[0061] In the present invention, the temperature of the preheated polytetrafluoroethylene mold is preferably 35-45°C.

[0062] In the present invention, the photocuring is preferably performed under ultraviolet light, and the photocuring time is preferably 2 minutes.

[0063] In the present invention, the wavelength of the ultraviolet light is preferably 365 nm, and the intensity is preferably 10 mW / cm 2 .

[0064] After the photocuring is completed, the present invention preferably further comprises naturally cooling to room temperature and then demoulding to obtain the shape memory polymer.

[0065] The present invention also provides the use of the near-infrared-magnetic response shape memory photocurable ink described in the above technical solution in the preparation of a blood vessel branch stent.

[0066] In the present invention, the preparation of the branch blood vessel stent preferably utilizes 3D printing technology to print the branch blood vessel stent according to a model designed by Blender software.

[0067] In the present invention, the 3D printing technology is preferably carried out under ultraviolet light irradiation conditions, the printing speed is preferably 50 to 60 s / layer, the number of layers is preferably 884 layers, and the height of a single layer is preferably 0.05 mm.

[0068] In order to further illustrate the present invention, the near-infrared-magnetic responsive shape memory photocurable ink provided by the present invention and its preparation method and application are described in detail below in combination with examples, but they should not be understood as limiting the scope of protection of the present invention.

[0069] Example 1

[0070] Weigh 0.6g of tris(hydroxymethyl)aminomethane) in a round-bottom flask, pour in 500mL of ultrapure water, and adjust the pH value of the solution to 8.5 with hydrochloric acid. Add 0.8g of Fe3O4 magnetic nanoparticles to the flask, and disperse them evenly in the solution by high-frequency ultrasound for 4h. The resulting solution is black. Add 1g of dopamine hydrochloride powder to the solution, stir mechanically for 24h at room temperature in the dark, pour the mixed solution into a beaker, let it stand for 30min, and place a strong magnet underneath to accelerate the sedimentation of Fe3O4 magnetic nanoparticles. Pour out the brown-black upper layer of liquid, and wash the lower black precipitate with ultrapure water and anhydrous ethanol several times until the washing liquid becomes light yellow and neutral. Finally, the resulting black precipitate is placed in a vacuum oven at 40℃ for 48h to obtain dopaminized Fe3O4 magnetic nanoparticles for later use.

[0071] Weigh 40g of polytetrahydrofuran and 6.72g of hexamethylene diisocyanate into a three-necked flask and dissolve them fully. Heat to 80°C, condense and reflux under a nitrogen atmosphere, and stir mechanically for 2h to carry out addition reaction to obtain an isocyanate-terminated prepolymer. Add 5.2g of hydroxyethyl methacrylate preheated to 80°C into a three-necked flask, and continue to stir mechanically for 2h under a nitrogen atmosphere. Pour the reacted sample into a glass reagent bottle while hot, put it into a 60°C vacuum oven to remove bubbles, and cool it to room temperature to obtain a prepolymer with an appearance of a white waxy solid, which is sealed and stored at room temperature.

[0072] Weigh 9g of prepolymer and mix it with 6g of hydroxyethyl methacrylate and 15g of dimethylaminoethyl methacrylate, and stir it mechanically in a 40℃ water bath and N2 atmosphere for 1h to ensure that the prepolymer is fully dissolved. Weigh 0.9g of dopaminated Fe3O4 magnetic nanoparticles and add them to the flask, and use high-frequency ultrasound for 2h to ensure that the particles are evenly dispersed. Then add 0.03g of inhibitor hydroquinone and 0.3g of photoinitiator (2,4,6-trimethylbenzamide) diphenylphosphine oxide (TPO), and continue stirring for 0.5h at 40℃, wrapped in tin foil to avoid light, to obtain a dark black photosensitive ink. Pour the obtained ink into preheated polytetrafluoroethylene molds and irradiate at a wavelength of 365nm and an intensity of 10mW / cm 2Under ultraviolet light irradiation, the cross-linking reaction was carried out for 2 minutes, and then the black shape memory polymer was obtained by demolding after cooling to room temperature.

[0073] Application Example 1

[0074] Using ANYCUBIC PHOTO printer ( Figure 4 A), the ink prepared in Example 1 is loaded into a material box, and the model designed by Blender software ( Figure 4 Middle B) Printing branch vascular stents, 3D printing under ultraviolet light irradiation, printing speed 50s / layer, printing 884 layers, single layer height 0.05mm, to obtain 4D printed multi-responsive branch vascular stents (structure as shown Figure 4 (as shown in C), the main body has a diameter of 16 mm and a length of 18 mm, and the branch has a diameter of 8 mm and a length of 20 mm.

[0075] Example 2

[0076] Weigh 0.6g of tris(hydroxymethyl)aminomethane) in a round-bottom flask, pour in 500mL of ultrapure water, and adjust the pH value of the solution to 8.5 with hydrochloric acid. Add 0.8g of Fe3O4 magnetic nanoparticles to the flask, and disperse them evenly in the solution by high-frequency ultrasound for 4h. The resulting solution is black. Add 1g of dopamine hydrochloride powder to the solution, stir mechanically for 24h at room temperature in the dark, pour the mixed solution into a beaker, let it stand for 30min, and place a strong magnet underneath to accelerate the sedimentation of Fe3O4 magnetic nanoparticles. Pour out the brown-black upper layer of liquid, and wash the lower black precipitate with ultrapure water and anhydrous ethanol several times until the washing liquid becomes light yellow and neutral. Finally, the resulting black precipitate is placed in a vacuum oven at 40℃ for 48h to obtain dopaminized Fe3O4 magnetic nanoparticles for later use.

[0077] Weigh 40g of polytetrahydrofuran and 6.72g of hexamethylene diisocyanate into a three-necked flask and dissolve them fully. Heat to 80°C, condense and reflux under a nitrogen atmosphere, and stir mechanically for 2h to carry out addition reaction to obtain an isocyanate-terminated prepolymer. Add 5.2g of hydroxyethyl methacrylate preheated to 80°C into a three-necked flask, and continue to stir mechanically for 2h under a nitrogen atmosphere. Pour the reacted sample into a glass reagent bottle while hot, put it into a 60°C vacuum oven to remove bubbles, and cool it to room temperature to obtain a prepolymer with an appearance of a white waxy solid, which is sealed and stored at room temperature.

[0078] Weigh 9g of prepolymer and mix with 10.5g of hydroxyethyl methacrylate and 10.5g of dimethylaminoethyl methacrylate, and stir mechanically for 1h in a 40℃ water bath under N2 atmosphere to ensure that the prepolymer is fully dissolved. Weigh 0.9g of dopaminated Fe3O4 magnetic nanoparticles and add them to the flask, and high-frequency ultrasound for 2h to ensure that the particles are evenly dispersed, then add 0.03g of inhibitor hydroquinone and 0.3g of photoinitiator DMPA, and continue stirring for 0.5h at 40℃, wrapped in tin foil to avoid light, to obtain a dark black photosensitive ink. Pour the obtained ink into preheated polytetrafluoroethylene molds and irradiate at a wavelength of 365nm and an intensity of 10mW / cm 2 Under ultraviolet light irradiation, the cross-linking reaction was carried out for 2 minutes, and then the black shape memory polymer was obtained by demolding after cooling to room temperature.

[0079] Application Example 2

[0080] Using an ANYCUBIC PHOTO printer, the ink prepared in Example 2 was loaded into a material box, and the 3D printing technology was used according to the model designed by Blender software ( Figure 4 Middle B) Printing branch vascular stents, 3D printing under ultraviolet light irradiation, printing speed 60s / layer, printing 884 layers, single layer height 0.05mm, to obtain 4D printed multi-responsive branch vascular stents (structure as shown Figure 4 (as shown in C), the main body has a diameter of 16 mm and a length of 18 mm, and the branch has a diameter of 8 mm and a length of 20 mm.

[0081] Example 3

[0082] Weigh 0.6g of tris(hydroxymethyl)aminomethane) in a round-bottom flask, pour in 500mL of ultrapure water, and adjust the pH value of the solution to 8.5 with hydrochloric acid. Add 0.8g of Fe3O4 magnetic nanoparticles to the flask, and disperse them evenly in the solution by high-frequency ultrasound for 4h. The resulting solution is black. Add 1g of dopamine hydrochloride powder to the solution, stir mechanically for 24h at room temperature in the dark, pour the mixed solution into a beaker, let it stand for 30min, and place a strong magnet underneath to accelerate the sedimentation of Fe3O4 magnetic nanoparticles. Pour out the brown-black upper layer of liquid, and wash the lower black precipitate with ultrapure water and anhydrous ethanol several times until the washing liquid becomes light yellow and neutral. Finally, the resulting black precipitate is placed in a vacuum oven at 40℃ for 48h to obtain dopaminized Fe3O4 magnetic nanoparticles for later use.

[0083] Weigh 40g of polytetrahydrofuran and 6.72g of hexamethylene diisocyanate into a three-necked flask and dissolve them fully. Heat to 80°C, condense and reflux under a nitrogen atmosphere, and stir mechanically for 2h to carry out addition reaction to obtain an isocyanate-terminated prepolymer. Add 5.2g of hydroxyethyl methacrylate preheated to 80°C into a three-necked flask, and continue to stir mechanically for 2h under a nitrogen atmosphere. Pour the reacted sample into a glass reagent bottle while hot, put it into a 60°C vacuum oven to remove bubbles, and cool it to room temperature to obtain a prepolymer with an appearance of a white waxy solid, which is sealed and stored at room temperature.

[0084] Weigh 9g of prepolymer and mix with 15g of hydroxyethyl methacrylate and 6g of dimethylaminoethyl methacrylate, and stir mechanically in a 40°C water bath under N2 atmosphere for 1h to ensure that the prepolymer is fully dissolved. Weigh 0.9g of dopaminated Fe3O4 magnetic nanoparticles and add them to the flask, and high-frequency ultrasound for 2h to ensure that the particles are evenly dispersed, then add 0.03g of inhibitor hydroquinone and 0.3g of photoinitiator (2,4,6-trimethylbenzamide) ethyl phosphonate, and continue stirring for 0.5h at 40°C, wrapped in tin foil to avoid light, to obtain a dark black photosensitive ink. Pour the obtained ink into preheated polytetrafluoroethylene molds and irradiate at a wavelength of 365nm and an intensity of 10mW / cm 2 Under ultraviolet light irradiation, the cross-linking reaction was carried out for 2 minutes, and then the black shape memory polymer was obtained by demolding after cooling to room temperature.

[0085] Application Example 3

[0086] Using an ANYCUBIC PHOTO printer, the ink prepared in Example 3 was loaded into a material box, and the 3D printing technology was used according to the model designed by Blender software ( Figure 4 Middle B) Printing branch vascular stents, 3D printing under ultraviolet light irradiation, printing speed 55s / layer, printing 884 layers, single layer height 0.05mm, to obtain 4D printed multi-responsive branch vascular stents (structure as shown Figure 4 (as shown in C), the main body has a diameter of 16 mm and a length of 18 mm, and the branch has a diameter of 8 mm and a length of 20 mm.

[0087] Comparative Example 1 (without dopaminated Fe3O4 magnetic nanoparticles)

[0088] Weigh 40g of polytetrahydrofuran and 6.72g of hexamethylene diisocyanate into a three-necked flask and dissolve them fully. Heat to 80°C, condense and reflux under nitrogen atmosphere, and stir mechanically for 2h to carry out addition reaction to obtain an isocyanate-terminated prepolymer. Add 5.2g of hydroxyethyl methacrylate preheated to 80°C into a three-necked flask, and continue to stir mechanically for 2h under nitrogen atmosphere. Pour the reacted sample into a glass reagent bottle while hot, put it into a 60°C vacuum oven to remove bubbles, cool to room temperature, and obtain a prepolymer with an appearance of white waxy solid, which is sealed and stored at room temperature. Weigh 9g of prepolymer and mix it with 15g of hydroxyethyl methacrylate and 6g of dimethylaminoethyl methacrylate, and stir mechanically for 1h in a 40°C water bath and N2 atmosphere to ensure that the prepolymer is fully dissolved. Add 0.03g of inhibitor hydroquinone and 0.3g of photoinitiator (2,4,6-trimethylbenzamide) diphenylphosphine oxide, and continue stirring for 0.5h at 40℃, wrapped in tin foil and protected from light to obtain colorless and transparent photosensitive ink. Pour the obtained ink into preheated polytetrafluoroethylene molds and heat at a wavelength of 365nm and an intensity of 10mW / cm 2 The cross-linking reaction was carried out for 2 minutes under ultraviolet light irradiation, and the mold was removed after cooling to room temperature to obtain a colorless and transparent shape memory polymer.

[0089] The mechanical properties of the shape memory polymer material were tested at room temperature using a Shimadzu AG-X (5000N) electronic universal testing machine, with a tensile speed of 10 mm / min, and the sample shape was cut into a dumbbell shape according to the international standard ISO-527-2 / 5B. It can be seen from the embodiments and comparative examples in Table 1 that the shape memory polymer obtained by the method of the present invention has good mechanical properties, and the mechanical properties can be regulated by adjusting the ratio of the prepolymer to the acrylate; more importantly, compared with the tensile strength and breaking rate of the great saphenous vein of human beings in the literature, the material obtained by the present invention has excellent mechanical properties and has broad prospects for medical applications.

[0090] Table 1 Comparison of mechanical properties between the examples and the comparative examples

[0091] Example 1 Example 2 Example 3 Comparative Example 1 Great saphenous vein Elongation at break (%) 64.8 118.3 201.3 170.5 242 Tensile strength(MPa) 22.1 21.1 20.8 18.1 1.8

[0092] Transmission electron microscopy was used to analyze the morphology of magnetic nanoparticles. Figure 1 Transmission electron microscopy images of agglomerated Fe3O4 magnetic nanoparticles without dopamine modification (left) and dopamine-modified Fe3O4 magnetic nanoparticles (right). Figure 1 It shows that the aggregation of Fe3O4 magnetic nanoparticles modified with dopamine is significantly reduced, and the dispersion is more uniform, which is conducive to uniform mixing in the photocurable ink; and the polydopamine layer coated on the surface of Fe3O4 magnetic nanoparticles gives the material excellent cross-linking and near-infrared response capabilities.

[0093] Differential scanning calorimetry analysis was performed on the ink photocured films in Example 3 and Comparative Example 1. Figures 2-3 As shown, Figure 2 The differential scanning calorimetry analysis curve of the ink photocured film in Comparative Example 1 is as follows: Figure 3 The differential scanning calorimetry curve of the ink photocured film in Example 3 was compared with the cured film without dopaminated Fe3O4 magnetic nanoparticles (49.2°C). The glass transition temperature of the polymer formed by photocuring in Example 3 was reduced to 37.7°C, which is suitable for human body temperature. This result proves that the prepared 4D printed multi-responsive medical intracavitary implant can be actually used in the human body to transform its shape and reduce surgical trauma.

[0094] The magnetic response and near infrared response performance of the material in Example 3 were tested using a neodymium iron boron magnet, a 3kHz alternating magnetic field coil and an 808nm laser transmitter. Figure 5 As shown: A. The spline obtained in Example 3 is slowly brought close to the magnet at room temperature, and it can be seen that the spline is attracted by the magnet. D. The sample obtained in Example 3 is cut into a "petal" shape, programmed into a "closed" shape in an 80°C hot water bath, quickly cooled to 0°C and fixed, and placed on a 3kHz alternating magnetic field coil at room temperature. It can be seen that the "petal" is completely "opened" within 30s and restores the original shape, indicating that the material has magnetic response ability. B. The spline obtained in Example 3 is programmed into a spiral vascular stent shape in an 80°C hot water bath, quickly cooled to 0°C and fixed, and near-infrared laser is used to irradiate different parts of the stent at room temperature. It can be seen that the near-infrared light irradiation area is obviously deformed and returns to its original shape after 16 seconds. C. Immediately after the test, the temperature of the stent is observed with an infrared imager. It can be seen that the central temperature is 41.4°C, which is higher than its transition temperature, and has a fast near-infrared response capability. The multiple response capabilities are expected to improve the shortcomings of the existing shape memory polymers that respond to single and irreversible deformation, expand their application in medical intracavitary grafts, and achieve complex deformation.

[0095] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing near-infrared-magnetic responsive shape memory photocurable ink, characterized in that: The following steps are involved: The polytetrahydrofuran and diisocyanate are mixed and subjected to addition reaction to obtain a prepolymer; The prepolymer and the first acrylate are mixed to carry out polymerization reaction to obtain a polyurethane prepolymer; The polyurethane prepolymer, the second acrylate, dopaminated Fe3O4 magnetic nanoparticles, an inhibitor and a photoinitiator are mixed to obtain the near-infrared-magnetic responsive shape memory photocurable ink; The mass ratio of the polyurethane prepolymer, the second acrylate, the dopaminated Fe3O4 magnetic nanoparticles, the inhibitor and the photoinitiator is 9:12-30:0.9:0.03:0.3-0.

6.

2. The preparation method according to claim 1, characterized in that: The first acrylate and the second acrylate independently include one or more of hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, methyl 2-methacrylate, and ethyl 2-methacrylate.

3. The preparation method according to claim 1, characterized in that: The dopaminated Fe3O4 magnetic nanoparticles have Fe3O4 magnetic nanoparticles as cores and polydopamine as shells. The mass ratio of the Fe3O4 magnetic nanoparticles to polydopamine is 0.8-1.6:1, and the particle size of the Fe3O4 magnetic nanoparticles is 50nm.

4. The preparation method according to claim 1, characterized in that: The mass ratio of the polytetrahydrofuran to the diisocyanate is 40:6.

72.

5. The preparation method according to claim 1 or 4, characterized in that: The mass ratio of the polytetrahydrofuran to the first acrylate is 40:5.

2.

6. The preparation method according to claim 1 or 4, characterized in that: The diisocyanate includes naphthalene diisocyanate, 4,4-diphenylmethane diisocyanate, toluene diisocyanate or hexamethylene diisocyanate.

7. The near-infrared-magnetic responsive shape memory photocurable ink prepared by the preparation method according to any one of claims 1 to 6.

8. Use of the near-infrared-magnetic responsive shape memory photocurable ink according to claim 7 in the preparation of shape memory polymers.

9. Use of the near-infrared-magnetic responsive shape memory photocurable ink according to claim 7 in the preparation of vascular branch stents.

Citation Information

Patent Citations

  • Polydopamine-coated nanometer composite photothermal reagent and preparation method thereof

    CN106421785A

  • Preparation method and applications of 3D printing composite magnetic metal scaffold

    CN107715182A

  • Preparation method of thermally reversible polyurethane composite material for 4D printing

    CN110922745A

  • Photosensitive resin and preparation method and application thereof

    CN111040102A

  • 4D (four-dimensional) printing light-cured cyanate printing ink, preparation method of 4D printing light-cured cyanate printing ink and shape memory cyanate material

    CN115627071A