A kind of strengthening treatment method of mica paper

The polyimide film layer obtained by surface corrosion treatment and specific combination reinforced fillers, combined with the modified fiber ratio, solve the defects in mechanical strength, temperature resistance and insulation properties of traditional mica paper, and prepare high mechanical strength, Mica paper with high temperature resistance and high insulation is suitable for high temperature environments and avoids the problem of complex process and increasing thickness.

CN116716754BActive Publication Date: 2024-11-22PINGJIANG SHENGYING MICA IND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310711542.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-15
Publication Date
2024-11-22
Estimated Expiration
2043-06-15

AI Technical Summary

Technical Problem

Traditional aramid mica paper has defects in mechanical strength, temperature resistance and insulation performance, especially in high temperature environments, which are prone to strength defects and deterioration of insulation performance, and the complex process increases the thickness of the finished product and affects the overall performance.

Method used

The polyimide film layer obtained by surface corrosion treatment is used as the intermediate dielectric layer, combined with a specific combination to enhance the ratio of fillers and modified fibers, and is prepared with high mechanical properties through circular mesh papermaking, bristle treatment, spraying and hot pressing forming processes. Mica paper with strength, high temperature resistance and high insulation.

Benefits of technology

It effectively makes up for the pores and strength defects of mica paper, improves mechanical, insulation and temperature resistance, is suitable for high adaptability in high temperature harsh environments, and avoids the negative gain of the traditional process to increase thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004287895750000061
    Figure BDA0004287895750000061
Patent Text Reader

Abstract

The present invention discloses a method for enhancing mica paper, which can be used to prepare mica paper products with a thickness between 0.08 and 0.30 mm. The method first prepares aramid mica paper pulp, and uses the aramid mica paper pulp to make a mica paper substrate, then performs surface roughening treatment on the rough surface of the mica paper substrate, and then takes a polyimide film layer, and uses weak alkali etching to obtain a polyimide film layer with a rough surface; sprays a combined reinforcing filler containing a specific sizing material and a combined filler on the rough surface of the mica paper substrate: then covers the prepared polyimide film layer on the surface of the combined reinforcing filler, and after hot pressing and forming into one, uses the mica paper substrate with a polyimide film layer as a basis, and makes a mica paper surface layer on its surface according to the thickness difference, and obtains the finished mica paper after drying and forming. The mica paper prepared by the present invention forms a stable cross-linked structure inside, and has good structural uniformity, high density, good electrical properties, and excellent tensile strength and thermal conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of insulating mica products, in particular to a reinforcing treatment method for producing mica paper with better physical properties. Background Art

[0002] In recent years, with the continuous development of my country's economy and scientific and technological progress, people's demand for electric energy has gradually increased, and the application of insulating materials in electrical equipment has also attracted people's attention. With the rapid development of power electronics technology and new semiconductor devices, the number of electrical equipment working in various complex engineering environments has increased day by day, which puts forward new requirements for the mechanical strength, temperature resistance, moisture resistance, corona resistance, and service life of traditional insulating materials.

[0003] Aramid mica paper products are a flexible thin paper-based insulating material prepared by wet papermaking technology. They are made by crushing and pulping the mica sheet raw materials, mixing them with aramid fibers, and then wet-papering them. They have the advantages of good temperature resistance, strong flame retardancy, high insulation performance, stable chemical properties, light weight and softness, low price and environmental friendliness. They are used as the main insulating material for electrical equipment such as variable frequency motors, high-power generators, and special transformers.

[0004] In the prior art, the product quality of aramid mica paper products is affected by many factors. In addition to being affected by the type, particle size, gradation of mica and the characteristics of the raw materials such as aramid fiber, it is also affected by the raw material ratio of the preparation process, the type and amount of dispersant. However, due to the material difference between aramid fiber and mica itself, there are large differences in surface properties and density, which makes the aramid mica paper produced under traditional process conditions have the problem of low interface strength. After long-term use, it is easy to have strength defects and even structural dissociation. At the same time, there are a large number of pores in the molded aramid mica paper. When an external voltage is applied, electrons can easily penetrate the paper through the pores, thereby affecting the insulation performance. In addition, the temperature resistance is poor. When continuously operated under high temperature conditions, the above insulation defects will continue to deteriorate. Although the above defects can be alleviated to a certain extent through process and material processing, the process is complicated, and the thickness of the finished mica paper will be increased, accompanied by some negative gains in comprehensive performance.

[0005] Therefore, it is an urgent need in this field to design a new mica paper preparation method to obtain mica paper with high mechanical strength, high temperature resistance, high insulation and high adaptability to harsh environments with continuous high temperatures. Summary of the invention

[0006] The technical problem solved by the present invention is to provide a method for enhancing mica paper to solve the shortcomings of the above-mentioned background technology.

[0007] The technical problem solved by the present invention is achieved by adopting the following technical solutions:

[0008] A method for enhancing mica paper, comprising the following steps:

[0009] S1: preparing aramid mica pulp, using the aramid mica pulp to make a mica paper substrate using a rotary paper machine according to the thickness of the mica paper to be processed at 1 / 2 to 2 / 3, and then performing a surface grinding treatment on the rough surface of the mica paper substrate to obtain a mica paper substrate with a single-sided rough surface;

[0010] S2 takes a polyimide film layer and performs surface corrosion treatment on it using an alkali solution to obtain a polyimide film layer with a rough surface;

[0011] S3 sprays the rough surface of the mica paper substrate obtained in step S1 with a composite reinforcing filler:

[0012] The combined reinforcing filler includes a rubber compound and a filler, wherein the mass proportion of the filler in the rubber compound is 7-12%; the filler is composed of reinforcing particles and reinforcing fibers in a mass ratio of 1:3-1:2, wherein the reinforcing particles are white carbon black and ultrafine graphite powder, and the reinforcing fibers are short-cut aramid fibers and polyaromatic oxadiazole fibers modified by soaking in sodium dodecylbenzene sulfonate, and the mass ratio of the two is 5:1-7:1;

[0013] S4: Covering the surface of the combined reinforcing filler with a polyimide film layer, and hot pressing to form the combined reinforcing filler into a whole;

[0014] S5 uses a mica paper substrate with a polyimide film layer as the basis, and manufactures a mica paper surface layer on its surface according to the thickness difference. After drying and forming, the finished mica paper is obtained.

[0015] As a further limitation, the aramid mica pulp material contains aramid fibers in an amount of 17 to 23% by mass, and the mass ratio of chopped fibers to precipitated fibers in the aramid fibers is 7:3 to 3:1;

[0016] The aramid mica pulp material is prepared by subjecting the aramid fiber to a modification treatment. During the modification treatment, the short-cut fibers are heated at 75 to 80°C and 0.7 to 0.9×10 -3 mol / L sodium dodecylbenzene sulfonate solution for 2-3 hours, take out and filter and dry; then use high-speed dispersing equipment to disperse the precipitated fibers, the dispersion time is 90min-120min, the front stage of the dispersion is carried out at a speed of 12000-15000 rpm, short-cut fibers are added to continue the dispersion when the dispersion time accounts for 30% of the total dispersion time, polyethylene oxide is added when the dispersion time accounts for 15% of the total dispersion time, and the equipment speed is reduced to 7000-9000 rpm until the dispersion is completed, so as to obtain an aramid fiber material with better dispersibility in the slurry;

[0017] In order to ensure the deflaking effect, the polyethylene oxide used for the above deflaking process is polyethylene oxide with a molecular weight of 2.7 to 4 million, and the addition amount is 0.3 to 0.5% relative to the absolute dry paper mass;

[0018] In order to ensure the decomposition effect, a quaternary ammonium salt accounting for 0.07-0.09% of the mass of the sodium dodecylbenzene sulfonate solution is also added to the sodium dodecylbenzene sulfonate solution in the above decomposition process.

[0019] As a further limitation, the chopped fibers in the aramid fiber material are preferably meta-aramid chopped fibers with a monofilament length of 2 to 5 mm and a monofilament diameter of 10 to 20 μm; and the precipitated fibers are preferably meta-aramid precipitated fibers with a length of 0.20 to 0.35 mm and a diameter of 15 to 18 μm.

[0020] As a further limitation, the thickness of the polyimide film layer is 30-50 μm.

[0021] As a further limitation, the white carbon black used in the combined reinforcing filler is fumed white carbon black.

[0022] As a further limitation, the ultrafine graphite powder used in the combined reinforcing filler is spherical graphite powder.

[0023] As a further limitation, the spraying treatment method of the combined reinforcing filler on the rough surface of the mica paper substrate is pressure spraying or electrostatic spraying.

[0024] As a further limitation, the adhesive used in the combined reinforcing filler is an epoxy resin adhesive with a softening point of 80 to 120° C., a viscosity of 22 to 28 Pa·s, and a relative molecular weight of 5000 to 8000.

[0025] Beneficial effects: The mica paper reinforcement processing method of the present invention improves on the traditional mica paper preparation process, and utilizes the polyimide film layer obtained by surface etching treatment as the intermediate medium layer to reinforce the mica paper substrate and the mica paper surface layer on both sides, and is particularly suitable for preparing mica paper products with a thickness between 0.08 and 0.30 mm.

[0026] The method utilizes a surface-corroded polyimide film layer to compensate for the pore defects in the aramid mica paper, and strengthens the interlayer structure through a specific combination of reinforcing fillers to compensate for the strength defects. At the same time, the combination of the polyimide film layer and the reinforcing particles can also effectively improve the mechanical, insulating and temperature-resistant properties of the aramid mica paper. By optimizing the ratio of aramid precipitated fibers to chopped fibers, the amount of additives added, and the mica content, a mica paper of a specific thickness that is soft, flame-resistant, and resistant to cold and heat is obtained. DETAILED DESCRIPTION

[0027] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below in conjunction with specific embodiments.

[0028] In the following embodiments, it will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical terms and scientific terms) used herein have the same meaning as the general understanding of those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have the same meaning as the meaning in the context of the prior art, and will not be interpreted with an idealized or overly formal meaning unless defined as herein.

[0029] In the examples, the aramid mica pulp used to prepare the finished mica paper of fixed thickness is prepared in the following manner:

[0030] First, prepare mica slurry, using mica flakes with a particle size greater than 0.6 mm, mica flakes with a particle size range of 0.4-0.6 mm, and mica flakes with a particle size less than 0.4 mm as raw materials to prepare mica slurry, control the mass ratio of the above three types of mica flakes in the mica slurry to be 1:4:3, and set the above mica slurry aside after preparation.

[0031] The mica flakes in the above ratio can make the mica paper have better tensile strength and dielectric properties under the combination performance of the mica flakes themselves when preparing mica slurry and papermaking the mica slurry to obtain mica paper.

[0032] Then treat the aramid fiber:

[0033] Select meta-aramid short fibers with a monofilament length of 2 to 5 mm and a monofilament diameter of 10 to 20 μm as short fibers, select meta-aramid fibrils with a length of 0.20 to 0.35 mm and a diameter of 15 to 18 μm as fibrils, and control the mass ratio of short fibers to fibrils to be 8:3. -3 The fibers were immersed in a mol / L sodium dodecylbenzene sulfonate solution for 2.5 h, filtered after immersion, and dried with warm air at 55° C. to obtain dry modified chopped fibers.

[0034] The precipitated fibers were debonded using a high-speed dispersing device. The entire debonding process took 100 minutes and was carried out in three steps:

[0035] Step 1: Process at a speed of 14500 rpm for 30 min;

[0036] Step 2: Maintain the rotation speed of step 1, add the modified chopped fibers, and continue the process for 15 minutes;

[0037] Step 3: Reduce the equipment speed to 8500 rpm, then add polyethylene oxide with a molecular weight of 2.7 to 4 million, and control the amount of polyethylene oxide added to 0.35% relative to the absolute dry paper mass. When adding polyethylene oxide, add it slowly and evenly within 5 minutes, and then maintain the reaction conditions and continue to process until the reaction is completed to obtain an aramid fiber with better dispersibility.

[0038] The obtained aramid fiber material is added into the mica slurry prepared by the above method, and the aramid mica paper slurry is obtained after being evenly dispersed.

[0039] Preparation of polyimide film layer for intermediate dielectric layer:

[0040] A commercially available polyimide film layer with a thickness of 50 μm was taken, and the surface of the polyimide film layer was subjected to low-concentration alkali corrosion treatment, and was placed in a 55° C., 0.08% mass concentration NaOH or KOH solution for treatment for 45 minutes to obtain a polyimide film layer with a corroded rough surface.

[0041] In other embodiments, the polyimide film layer may be subjected to alkaline corrosion treatment by treating it in a NaOH or KOH solution with a mass concentration of 0.08-3% and a temperature of 50-65° C. for 30-50 minutes to obtain similar effects.

[0042] Preparation of composite reinforcing fillers:

[0043] Fumed silica and spherical graphite powder are selected as reinforcing particles, wherein the particle size of the fumed silica is 0.050-0.080 μm, and the particle size of the spherical graphite powder is 6-8 μm. The fumed silica and the spherical graphite powder are mixed in a mass ratio of 1:8 to obtain the reinforcing particles in the combined reinforcing filler; in other embodiments, inorganic particles with better heat dissipation performance and physical strength, such as BN, SiN, SiC, etc., can also be added to the combined reinforcing filler to obtain the corresponding filling reinforcement effect.

[0044] The meta-aramid short-cut fibers with a monofilament length of 2 to 5 mm and a monofilament diameter of 10 to 20 μm and the short-cut polyaromatic oxadiazole fibers are selected and mixed in a mass ratio of 6:1 to obtain a composite fiber, and the composite fiber is modified by soaking in sodium dodecylbenzene sulfonate. The soaking process is carried out at 60°C and 1.5×10 - 3 The immersion process is carried out in a mol / L sodium dodecylbenzene sulfonate solution for 90 minutes. After the immersion is completed, the reinforcing fibers in the combined reinforcing filler are obtained.

[0045] The reinforcing particles and reinforcing fibers are mixed at a mass ratio of 1:3, and the mixture is added to an epoxy resin adhesive with a softening point of 80 to 120° C., a viscosity of 26 Pa·s, and a relative molecular weight of 6000 to 6500, and then dispersed evenly to obtain a finished composite reinforcing filler.

[0046] After the above raw materials are prepared, the mica paper can be prepared:

[0047] First, the corresponding aramid mica pulp is used to make a mica paper substrate by using a rotary paper machine according to the basis of 1 / 2 to 2 / 3 of the thickness of the mica paper to be processed. The mica paper substrate is a single layer of mica paper, and the single layer of mica paper obtained by the rotary paper machine has a smooth surface and a rough surface. The rough surface is subjected to a flat sanding device to obtain a mica paper substrate with a single-side rough surface;

[0048] The combined reinforcing filler prepared by the above method is sprayed on the rough surface of the mica paper substrate, the combined reinforcing filler is evenly coated on the rough surface of the mica paper substrate by electrostatic spraying, and then covered with a polyimide film layer, the polyimide film layer is covered on the surface of the combined reinforcing filler and then hot-pressed into a whole, and then the mica paper substrate with the polyimide film layer is used as a basis, and a mica paper surface layer is made on its surface according to the thickness difference, and the finished mica paper is obtained after drying and forming.

[0049] Based on the above method, the feeding process parameters are controlled to prepare mica paper of different thicknesses, and then the prepared mica paper is used as different embodiments for performance parameter detection, and the data are as follows (in order to reduce the influence of process parameters, especially the hot pressing composite process on the performance parameter value, the hot pressing composite temperature in different embodiments is set to 120° C., the hot pressing pressure is set to 12 MPa, and the hot pressing composite speed is set to 3 m / min in the hot pressing composite process):

[0050]

[0051] Based on the above table, it can be found that the mica paper prepared by the method of this embodiment has high mechanical strength, high temperature resistance, high insulation and high adaptability in harsh environments of continuous high temperature, and the mica paper of this embodiment has a slight improvement in tensile strength and thermal conductivity compared to traditional commercially available mica paper.

[0052] The reasons for obtaining the above performance are:

[0053] As for aramid mica pulp, as the content of aramid chopped fibers increases, the tensile strength index of aramid mica paper first increases and then decreases. This is because when the content of fibrils is high, the strength of the chopped fibers dominates the paper strength. When the content of fibrils decreases, the bonding force between fibers dominates the paper strength. By controlling the ratio of aramid fibrils to chopped fibers and testing different fiber ratios, it was found that when the ratio of fibrils to chopped fibers is 7:3, the optimal tensile strength is achieved through the synergistic effect of the high strength and high modulus of the chopped fibers themselves and the coating and bonding of the fibrils.

[0054] However, under the above fiber ratio conditions, the tensile strength can only be obtained by increasing the mass proportion of aramid fiber in the aramid mica pulp. This is why the aramid fiber content in many aramid mica papers increases from 30% to more than 30%. Although the increase in the proportion of aramid fiber can improve the tensile strength of mica paper, it will lead to a decrease in insulation performance.

[0055] In the present embodiment, the chopped fibers are modified and soaked in a sodium dodecylbenzene sulfonate solution of a specific concentration, and then the modified chopped fibers after the soaking treatment and the precipitated fibers are subjected to a high-temperature three-stage dispersion. This treatment method can obtain aramid fibers with better dispersibility in the slurry, prevent the aramid fibers from aggregating and flocculating in the aramid mica paper slurry, thereby reducing the amount of aramid fibers used, and cause the above-mentioned "the aramid chopped fiber content increases, and the tensile strength index of the aramid mica paper first increases and then decreases" change curve to lag behind, so as to accommodate more chopped fibers in the fiber cross-linking system, so that the tensile strength of the finished mica paper can be further improved due to the above-mentioned additionally accommodated chopped fibers, thereby achieving the effect of improved tensile strength.

[0056] Using an alkaline solution to perform surface corrosion treatment on the polyimide film layer can hydrolyze the imide-based surface layer into an imide metal salt, increase the surface roughness and surface active groups of the polyimide film layer, improve its hydrophilicity and adhesion, and the degree of hydrolysis increases with the increase of temperature and alkali solution concentration. By controlling the alkali solution concentration and reaction time, the polyimide film layer can obtain the above-mentioned surface modification properties while the overall physical and chemical properties of the polyimide film layer do not change much. The polyimide film layer obtained by the above-mentioned modification treatment method can be used to enhance the bonding performance of the polyimide film layer and the components in the combined reinforcing filler when pressed together, so that it can be combined with the aramid fiber in the aramid mica paper pulp and the reinforcing fiber in the combined reinforcing filler on both sides, thereby ensuring its anti-peeling performance at the interlayer interface. At the same time, the polyimide film layer can also be used to block a large number of pores in the aramid mica paper to prevent electrons from easily penetrating the paper through the pores when an external voltage is applied, thereby affecting the insulation performance of the mica paper after molding.

[0057] The contribution of this embodiment to the existing process also lies in the combined use of short-cut aramid fibers and polyaromatic oxadiazole fibers as reinforcing fibers in the combined reinforcing filler, wherein the full name of polyaromatic oxadiazole is aromatic poly-1,3,4-oxadiazole, referred to as POD, and the benzene rings and oxadiazole rings in its molecular chain are arranged alternately. It has excellent high temperature resistance, dimensional stability and thermal stability, can adapt to the working conditions of 250°C for a long time, and can still maintain good dimensional stability when the temperature is higher than 400°C. At the same time, it has a flame retardant functional group and has permanent flame retardancy without the need to add a flame retardant. The polyaromatic oxadiazole fibers are mixed with short-cut aramid fibers, and when modified by soaking in sodium dodecylbenzene sulfonate, they form a structurally stable cross-linked network with large and small space gaps with the short-cut aramid fibers. The large and small space gaps formed by this cross-linked network can be used as a grid to accommodate white carbon black and ultrafine graphite powder respectively and prevent them from escaping to form a stable structure, so that the mica paper forms a flame-resistant, cold and heat-resistant interlayer structure system in the interlayer reinforcement area.

[0058] In order to further optimize the crosslinking system of polyaromatic oxadiazole fiber and short-cut aramid fiber and the bonding performance of aramid fiber in aramid mica pulp, quaternary ammonium salt accounting for 0.07-0.09% of the mass of sodium dodecylbenzene sulfonate solution can also be added to the sodium dodecylbenzene sulfonate solution in the above-mentioned modification process and the aramid mica pulp decomposition process.

[0059] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for enhancing mica paper, characterized in that: The specific processing steps include: S1: preparing aramid mica pulp, using the aramid mica pulp to make a mica paper substrate using a rotary paper machine according to 1 / 2 to 2 / 3 of the thickness of the mica paper to be processed, and then performing a surface grinding treatment on the rough surface of the mica paper substrate to obtain a mica paper substrate with a single-side rough surface; The aramid mica pulp material contains aramid fibers in a mass ratio of 17 to 23%, and the mass ratio of short-cut fibers to precipitated fibers in the aramid fibers is 7:3 to 3:1; The aramid mica pulp material is prepared by subjecting the aramid fiber to a modification treatment. During the modification treatment, the short-cut fibers are heated at 75-80°C and 0.7-0.9×10 -3 mol / L sodium dodecylbenzene sulfonate solution for 2-3 hours, take out and filter and dry; then use high-speed dispersing equipment to disperse the precipitated fibers, the dispersion time is 90min-120min, the front stage of the dispersion is carried out at a speed of 12000-15000 rpm, and when the dispersion time accounts for 30% of the total dispersion time, short-cut fibers are added to continue the dispersion, and when the dispersion time accounts for 15% of the total dispersion time, polyethylene oxide is added, and the equipment speed is reduced to 7000-9000 rpm until the dispersion is completed, so as to obtain an aramid fiber material with better dispersibility in the slurry; S2 takes a polyimide film layer and performs surface corrosion treatment on it using an alkali solution to obtain a polyimide film layer with a rough surface; S3 sprays the rough surface of the mica paper substrate obtained in step S1 with a composite reinforcing filler: The combined reinforcing filler includes a rubber compound and a filler, wherein the mass ratio of the filler in the rubber compound is 7-12%; the filler is composed of reinforcing particles and reinforcing fibers in a mass ratio of 1:3-1:2, wherein the reinforcing particles are white carbon black and ultrafine graphite powder, and the reinforcing fibers are short-cut aramid fibers and polyaromatic oxadiazole fibers modified by soaking in sodium dodecylbenzene sulfonate, and the mass ratio of the two is 5:1-7:1; S4: Covering the surface of the combined reinforcing filler with a polyimide film layer, and hot pressing to form the combined reinforcing filler into a whole; S5 uses a mica paper substrate with a polyimide film layer as the basis, and manufactures a mica paper surface layer on its surface according to the thickness difference. After drying and forming, the finished mica paper is obtained.

2. The method for enhancing mica paper according to claim 1, characterized in that: The polyethylene oxide has a molecular weight of 2.7 to 4 million, and the added amount is 0.3 to 0.5% relative to the absolute dry paper mass.

3. The method for enhancing mica paper according to claim 1, characterized in that: The sodium dodecylbenzene sulfonate solution is further added with a quaternary ammonium salt accounting for 0.07-0.09% of the mass of the sodium dodecylbenzene sulfonate solution.

4. The method for enhancing mica paper according to claim 1, characterized in that: The chopped fibers in the aramid fiber material are preferably meta-aramid chopped fibers with a monofilament length of 2-5 mm and a monofilament diameter of 10-20 μm; and the precipitated fibers are preferably meta-aramid precipitated fibers with a length of 0.20-0.35 mm and a diameter of 15-18 μm.

5. The method for enhancing mica paper according to claim 1, characterized in that: The white carbon black used in the combined reinforcing filler is fumed white carbon black.

6. The method for enhancing mica paper according to claim 1, characterized in that: The ultrafine graphite powder used in the combined reinforcing filler is spherical graphite powder.

7. The method for enhancing mica paper according to claim 1, characterized in that: The spraying treatment method of the combined reinforcing filler on the rough surface of the mica paper substrate is pressure spraying or electrostatic spraying.

8. The method for enhancing mica paper according to claim 1, characterized in that: The adhesive used in the combined reinforcing filler is an epoxy resin adhesive with a softening point of 80-120° C., a viscosity of 22-28 Pa·s, and a relative molecular weight of 5000-8000.

Citation Information

Patent Citations

  • Preparation method of high-performance POD aramid fiber composite paper

    CN106245392A

  • High-wear-resistance mica paper adhesive tape and preparation method thereof

    CN111471407A

  • High-strength composite mica paper and preparation method thereof

    CN111485456A

  • Method for improving interface bonding strength of aramid fiber mica paper