A method for preparing enhanced bio-based lightweight aggregate

By removing oil stains on the surface of bio-based materials, heat treatment and roll-coated modified slurry treatment, a dense coating is generated, which solves the problems of weak interface connection and fiber corrosion in the application of bio-based light aggregates in concrete, and improves its mechanical properties and durability and realize the efficient utilization of concrete waste, reducing environmental pollution and production costs.

CN116730641BActive Publication Date: 2024-11-26HUAXIN CEMENT CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310566927.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-26
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

When used in concrete, existing bio-based light aggregates are used in concrete, due to the hydrophobicity of surface oily substances and the corrosion of fiber components in humid environments, the interface transition zone connection is weak, and the strength and durability are insufficient. At the same time, waste slurry resources in concrete production are wasted. and environmental pollution problems have not been effectively resolved.

Method used

The surface oil stain of bio-based materials is removed by sodium hydroxide solution, the surface structure is improved by heat treatment, and the interface modified slurry is prepared by concrete waste for roll coating. CO2 is introduced during the roll coating process to generate nano-to-submicron CaCO3 particles, forming Dense coatings to improve the mechanical properties and corrosion resistance of bio-based light aggregates.

Benefits of technology

It significantly improves the mechanical properties and corrosion resistance of bio-based light aggregates, reduces water absorption and elastic modulus, realizes the comprehensive resource utilization of bio-based materials and concrete waste, and reduces environmental pollution and production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for preparing an enhanced bio-based lightweight aggregate, which is characterized by comprising the following steps: soaking waste bio-based materials in a sodium hydroxide solution to remove oily impurities on the surface; taking out and drying, pouring into a crusher for crushing, and then screening with a screen; heat-treating the screened bio-based materials to improve their surface structure; pouring the heat-treated product into a rotating drum container, and adding an interface modified slurry for roll coating, and continuously introducing CO2 during the rolling coating process; the bio-based materials of the invention are derived from waste shells of crops and the like, and the enhanced interface modified slurry is waste generated in the production process of a concrete enterprise, and a series of modification treatments are performed on the bio-based materials to achieve comprehensive resource utilization of the bio-based materials and concrete waste.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a method for preparing a bio-based lightweight aggregate. Background Art

[0002] Lightweight aggregate has the advantages of low bulk density, thermal insulation, high strength, and corrosion resistance. It is widely used and studied in the field of building materials, especially in the lightweight concrete industry. With the increasing number of super-high-rise buildings in modern society and the rapid development of prefabricated structures, the demand for lightweight concrete is also increasing, and the quality requirements for lightweight aggregate are becoming more and more stringent. Natural lightweight aggregates are beginning to be in short supply. Natural lightweight aggregates are mostly derived from porous rocks, and large-scale mining will have an adverse impact on the environment. In the current context of increased environmental awareness among citizens and increasingly stringent environmental policies, finding renewable green lightweight aggregates to replace natural lightweight aggregates has become a research hotspot.

[0003] Bio-based aggregates are naturally characterized by low density and high firmness. However, the greasy substances attached to their surface are hydrophobic, which is not conducive to their direct application in concrete. In addition, the fiber components on the surface of bio-based aggregates will be corroded in a humid environment, with high water absorption and low elastic modulus, resulting in a weak connection between the interface transition zone between the surface and the cement stone. The prepared lightweight concrete has shortcomings in strength and durability. At the same time, in concrete production companies, the concrete waste slurry from cleaning mixer trucks and mixers contains a large amount of CSH gel and unhydrated cement and mineral admixtures. Direct disposal will cause a waste of resources and harm the environment.

[0004] Patent CN114409292A discloses a reinforcement layer, a reinforced lightweight aggregate, and a preparation method and application thereof. This method uses the characteristics of the reinforcement layer with high carbonization activity to compositely reinforce the surface of traditional lightweight aggregate. The quality of the lightweight aggregate prepared by this method is related to the thickness and uniformity of the surface reinforcement layer slurry; at the same time, the cost of mineralized cementitious materials and carbon mineralization enhancers should also be considered. Patent CN103496866A discloses a core-shell type sulphoaluminate cement-based high-strength lightweight aggregate and a preparation method thereof. This method forms a porous shell layer on the surface of fly ash ceramsite by coating sulphoaluminate cement-based cementitious materials on the outside of fly ash ceramsite to improve the strength of the lightweight aggregate. In this method, fly ash ceramsite is an artificial lightweight aggregate, and the cementitious material coating increases the production cost of lightweight aggregate. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing an enhanced bio-based lightweight aggregate. The bio-based material comes from the waste shells of crops and the like, and the enhanced interface modified slurry is the waste generated in the production process of a concrete enterprise. By performing a series of modification treatments on the bio-based material, the comprehensive resource utilization of the bio-based material and concrete waste is achieved.

[0006] In order to achieve the above purpose, the technical solutions adopted are as follows:

[0007] A method for preparing enhanced bio-based lightweight aggregate comprises the following steps:

[0008] (1) Soaking the waste bio-based materials in a sodium hydroxide solution to remove surface oily impurities;

[0009] (2) Take out and dry, pour into a crusher for crushing, and then use a screen to screen;

[0010] (3) heat treating the screened bio-based material to improve its surface structure;

[0011] (4) Pour the heat-treated product into a rotating drum container, add the interface modification slurry and perform roller coating, and continuously introduce CO2 during the roller coating process.

[0012] In the above scheme, the bio-based material in step 1 is any one of oil palm shell, palm tree shell, coconut shell, peach shell or a mixture thereof; the age is 5-10 years, and the apparent density is 1330-1400 kg / m 3 .

[0013] In the above scheme, the concentration of the sodium hydroxide solution in step 1 is 0.01% to 0.07%, the pH value is 10 to 13, and the soaking time is 12h to 24h.

[0014] In the above scheme, the particle sizes after screening in step 2 are 5-20 mm and 0-5 mm respectively.

[0015] In the above scheme, the heat treatment temperature in step 3 is set to 60°C to 80°C, and the time is 30min to 40min.

[0016] In the above scheme, the interface modification slurry in step 4 is prepared by mixing concrete waste, water and a dispersant;

[0017] The concrete waste is wastewater generated by cleaning concrete mixers, filter presses or concrete tankers, or waste slurry sediment generated by decomposition of waste concrete, and its dry basis composition contains CaO 40-50wt%, SiO2 30-40wt%, and the rest are unavoidable impurities;

[0018] The mass ratio of water to concrete waste dry basis is (1-2): 1; the dispersant is polycarboxylate, and the dosage is 0.2%-0.4% of the total mass of the interface modified slurry.

[0019] In the above scheme, the mass ratio of the interface modification slurry to the heat treatment product in the roller coating process in step 4 is 1:(5-8).

[0020] In the above scheme, the speed of the roller coating process in step 4 is 100rpm-200rpm, and the roller coating time is 1h to 1.5h.

[0021] In the above scheme, the flow rate of CO2 gas introduced in the roller coating process in step 4 is 2-4 L / min, and the concentration is 80-100 vol%.

[0022] In the above scheme, a 0.4-0.6 mm thick coating is formed on the surface of the enhanced bio-based lightweight aggregate obtained in step 4.

[0023] Bio-based aggregate is a natural agricultural production waste with the characteristics of light weight and high hardness. However, its application in the concrete industry is limited by the hydrophobicity of the greasy substances attached to its surface and the poor corrosion resistance of the fiber components of the surface shell. The present invention first uses NaOH solution to remove the oil stains on the surface of the bio-based aggregate to avoid uneven rolling of the coating material during the subsequent modification process caused by the oil stains; by heat-treating the surface of the bio-based aggregate, the surface fibers are partially inactivated, the content of weak components in the surface shell is reduced, the surface coating structure is improved, and the surface fibers are prevented from being corroded in a humid environment, thereby improving the bonding strength of the transition zone between the surface of the bio-based lightweight aggregate and the cement stone interface, and optimizing the mechanical properties and shrinkage properties of the concrete; the heat treatment retains a certain toughness and strength of the internal part of the fiber on the surface of the bio-based aggregate, and improves its crack resistance to a certain extent.

[0024] In order to improve the performance of the bio-based aggregate, the present invention further modifies it. First, the surface of the bio-based aggregate is rolled with concrete waste slurry. Concrete waste slurry contains CSH gel, unhydrated cement and mineral admixtures. Since the chemical composition is similar to that of cement hydration products, the potential risks caused by incompatibility can be avoided. Polycarboxylate dispersants are used to improve the uniformity and stability of the bio-based aggregate coating. Through the carbonization process, the concrete waste slurry on the surface of the bio-based aggregate reacts with CO2 to generate nano to submicron CaCO3 particles and silicone gel in the native position. On the one hand, because the coating is evenly applied, the generated CaCO3 particles are also evenly dispersed on the surface. CaCO3 particles act as induced crystal nuclei to accelerate the hydration process, and the hydration products are evenly distributed on the surface of the bio-based aggregate, which is beneficial to improving the homogeneity of the bio-based aggregate. At the same time, CaCO3 particles and hydration products are attached to the surface of the bio-based aggregate, making the surface more compact, strengthening the mechanical properties of the bio-based lightweight aggregate, and at the same time, the water absorption rate of the bio-based lightweight aggregate is reduced, the elastic modulus is increased, and the performance of the bio-based lightweight aggregate is optimized.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1) The present invention uses bio-based aggregates discarded in agricultural production as primary lightweight aggregates, which has the benefits of solid waste utilization and saving construction costs, reduces the damage to the environment caused by its accumulation, reduces the industry's carbon footprint, and promotes the sustainable development of concrete; fully utilizes the advantages of concrete waste slurry containing CSH gel and unhydrated minerals, while also avoiding the potential hazards of compatibility reactions; adopts rolling and carbonization processes to achieve high added value utilization of concrete waste slurry, produces economic and environmental benefits for waste in the concrete industry, and promotes the green development of the concrete industry.

[0027] 2) The comprehensive performance of bio-based lightweight aggregate is significantly improved through alkali washing, heat treatment, rolling coating and carbonization processes. Sodium hydroxide solution removes hydrophobic substances such as oil on the surface of bio-based aggregate, increasing the possibility of concrete waste slurry coating the surface of bio-based aggregate; heat treatment retains the original structure of natural macromolecules as much as possible, thereby improving the corrosion resistance of bio-based aggregate, and has the advantages of no chemical use, environmental friendliness, and low operating cost; dispersant improves the uniformity of concrete waste slurry coating; carbonization method produces nano to submicron CaCO3 particles in situ, which is lower in cost and better in dispersibility than directly adding nano calcium carbonate; the generated CaCO3 particles have a higher specific surface area, which promotes the hydration of low-calcium cement more significantly, enhances the direct bonding between cement paste and aggregate, reduces cracks, makes the microstructure of the bio-based lightweight aggregate shell generation layer more compact, reduces the water absorption rate of lightweight aggregate, increases the elastic modulus of lightweight aggregate, and stabilizes the quality. DETAILED DESCRIPTION

[0028] The following examples further illustrate the technical solution of the present invention, but are not intended to limit the scope of protection of the present invention.

[0029] A specific embodiment provides a method for preparing an enhanced bio-based lightweight aggregate, comprising the following steps:

[0030] (1) Soaking the waste bio-based materials in a sodium hydroxide solution to remove surface oily impurities;

[0031] (2) Take out and dry, pour into a crusher for crushing, and then use a screen to screen;

[0032] (3) heat treating the screened bio-based material to improve its surface structure;

[0033] (4) The heat-treated product is poured into a rotating drum container, and the interface modification slurry is added for roller coating. During the roller coating process, CO2 is continuously introduced, and a 0.4-0.6 mm thick coating is formed on the surface of the enhanced bio-based lightweight aggregate.

[0034] Specifically, the bio-based material in step 1 is any one of oil palm shell, palm tree shell, coconut shell, peach shell or a mixture thereof; the age is 5-10 years, and the apparent density is 1330-1400 kg / m 3 .

[0035] Specifically, the concentration of the sodium hydroxide solution in step 1 is 0.01% to 0.07%, the pH value is 10 to 13, and the soaking time is 12h to 24h.

[0036] Specifically, the particle sizes after screening in step 2 are 5-20 mm and 0-5 mm respectively.

[0037] Specifically, in step 3, the heat treatment temperature is set to 60° C. to 80° C., and the time is 30 min to 40 min.

[0038] Specifically, the interface modification slurry in step 4 is prepared by mixing concrete waste, water, and a dispersant;

[0039] The concrete waste is wastewater generated by cleaning concrete mixers, filter presses or concrete tankers, or waste slurry sediment generated by decomposing waste concrete, and its dry basis components contain 40-50wt% CaO, 30-40wt% SiO2, and the rest are inevitable impurities; the mass ratio of water to the dry basis of concrete waste is (1-2): 1; the dispersant is polycarboxylate, and the dosage is 0.2%-0.4% of the total mass of the interface modified slurry.

[0040] Specifically, in step 4, the mass ratio of the interface modified slurry to the heat-treated product in the roller coating process is 1:(5-8); the rate of the roller coating process is 100rpm-200rpm, and the roller coating time is 1h-1.5h; the flow rate of the CO2 gas is 2-4L / min, and the concentration is 80-100vol%.

[0041] The bio-based materials used in the following specific embodiments are the discarded materials after palm oil is extracted from oil palm trees. The dry basis of the concrete waste contains: CaO 42%, SiO2 40%, and other substances (including Al2O3, Fe2O3, SO3, MgO, K2O, Na2O and other inevitable impurities) 18%. The concentration of the NaOH solution is 0.02%, and the pH value is 12. The dispersant is BP-5040 polycarboxylate.

[0042] Example 1

[0043] (1) Weigh 2 kg of discarded oil palm shells and soak them in sodium hydroxide solution for 24 h to remove surface oily impurities;

[0044] (2) taking out the soaked oil palm shell and draining the excess liquid thereon, keeping the surface of the oil palm shell absolutely dry, pouring the oil palm shell into a crusher for crushing, and then screening with a sieve;

[0045] (3) placing the sieved oil palm shell aggregate into a heat treatment furnace, setting the temperature to 80° C. and the heat treatment time to 30 min;

[0046] (4) Weigh 200 g of concrete waste, 200 g of water, and 1.2 g of dispersant, and stir them evenly to form concrete waste slurry;

[0047] (5) Pour the oil palm shell aggregate into a rotating drum container, add waste concrete slurry and roll-coat at a speed of 200 rpm for 1 h; during the rolling process, continuously introduce CO2 gas at a concentration of 99.9 vol% and a flow rate of 2 L / min.

[0048] Example 2

[0049] The preparation of the enhanced oil palm shell lightweight aggregate is different from that in Example 1 in that the heat treatment temperature is set at 60° C. and the heat treatment time is 40 min.

[0050] Example 3

[0051] The preparation of the enhanced oil palm shell lightweight aggregate is different from that in Example 1 in that the rolling coating time is 1.5 h.

[0052] Example 4

[0053] The preparation of the enhanced oil palm shell lightweight aggregate is different from that in Example 1 in that the CO2 flow rate is 4 L / min.

[0054] Comparative Example 1

[0055] The preparation of the enhanced oil palm shell lightweight aggregate is different from that in Example 1 in that there is no heat treatment process.

[0056] Comparative Example 2

[0057] The preparation of the enhanced oil palm shell lightweight aggregate is different from that of Example 1 in that there is no roller coating process.

[0058] Comparative Example 3

[0059] The preparation of the enhanced oil palm shell lightweight aggregate is different from that of Example 1 in that there is no carbonization treatment process.

[0060] Comparative Example 4

[0061] The preparation of the enhanced oil palm shell lightweight aggregate is different from that in Example 1 in that the heat treatment temperature is 100°C.

[0062] The lightweight aggregates prepared in Examples 1 to 4 and Comparative Examples 1 to 4 were tested for bulk density, cylinder compressive strength and water absorption with reference to "Lightweight Aggregates and Test Methods Thereof GB / T17431.2-2010"; the results are shown in Table 1.

[0063] Table 1

[0064] sample <![CDATA[Bulk density / kg / m 3 > Cylinder pressure strength / MPa 1h water absorption rate / % Example 1 612 5.1 14 Example 2 593 4.3 12 Example 3 653 6.1 10 Example 4 632 5.9 13 Comparative Example 1 583 2.3 21 Comparative Example 2 563 3.1 17 Comparative Example 3 553 2.0 22 Comparative Example 4 583 3.5 18

[0065] Combining Comparative Examples 1 and 4 with Examples 1-4 and Table 1, it can be seen that the cylinder compression strength of Comparative Examples 1 and 4 is significantly lower than that of Examples 1-4, and the 1h water absorption rate is greater than that of Examples 1-4, indicating that the thermal pretreatment of the oil palm shell improves the surface activity, effectively prevents the shrinkage deformation caused by the water absorption of the oil palm shell lightweight aggregate, and at the same time improves the bonding strength between the cement stone and the oil palm shell lightweight aggregate, and improves the corrosion resistance of the oil palm shell lightweight aggregate in a humid environment.

[0066] Combining Comparative Example 2 with Examples 1-4 and Table 1, it can be seen that the cylinder pressure strength of Comparative Example 2 is significantly lower than that of Examples 1-4, and the 1h water absorption rate is greater than that of Examples 1-4, indicating that rolling pretreatment of the surface of the oil palm shell lightweight aggregate with concrete waste slurry can enhance the strength of the oil palm shell lightweight aggregate and reduce the water absorption rate of the oil palm shell lightweight aggregate.

[0067] Combining Comparative Example 3 with Examples 1-4 and Table 1, it can be seen that the cylinder pressure strength of Comparative Example 3 is significantly lower than that of Examples 1-4, and the 1h water absorption rate is greater than that of Examples 1-4, indicating that the nano to submicron CaCO3 particles generated by the pre-carbonization process of the oil palm shell lightweight aggregate are wrapped in the outer shell, optimizing the strength and water absorption performance of the lightweight aggregate.

[0068] The above results show that the enhanced bio-based lightweight aggregate prepared in Examples 1 to 4 has high strength and low water absorption; by recycling solid waste in production, the oil palm shell is first subjected to high-temperature heat treatment for deactivation, and then a concrete slurry coating rich in calcium ions is rolled on the surface, and finally carbonization reinforcement is performed. After multi-level modification treatment, the corrosion resistance and strength of the bio-based lightweight aggregate are improved, effectively taking into account the green and excellent performance characteristics of the lightweight aggregate, and having important economic and environmental benefits.

[0069] The above embodiments are only examples for clear explanation, and are not intended to limit the implementation methods. For ordinary technicians in the relevant field, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here, so the obvious changes or modifications derived are still within the protection scope of the invention.

Claims

1. A method for preparing enhanced bio-based lightweight aggregate, characterized in that The steps include: (1) Soaking the waste bio-based materials in sodium hydroxide solution to remove oily impurities on the surface; the bio-based materials are any one of palm tree shells, coconut shells, peach shells or a mixture thereof; the age is 5-10 years, and the apparent density is 1330-1400 kg / m 3 ; (2) Take it out and dry it, pour it into a crusher for crushing, and then use a screen to screen it; (3) heat treating the screened bio-based material at 60°C to 80°C for 30 min to 40 min to improve its surface structure; (4) pouring the heat-treated product into a rotating drum container, adding the interface modification slurry for roll coating, and continuously introducing CO2 during the roll coating process; The interface modification slurry is prepared by mixing concrete waste, water and dispersant; the mass ratio of water to concrete waste on a dry basis is (1-2): 1; the dispersant is a polycarboxylate, and the dosage is 0.2%-0.4% of the total mass of the interface modification slurry; the concrete waste is wastewater generated by cleaning a concrete mixer, a filter press or a concrete tanker, or waste slurry precipitate generated by decomposition of waste concrete, and the dry basis components thereof contain 40-50wt% CaO, 30-40wt% SiO2, and the rest are unavoidable impurities; The mass ratio of the interface modified slurry to the heat-treated product in the roller coating process is 1:(5~8); the speed of the roller coating process is 100rpm-200rpm, and the rolling time is 1h~1.5h; the flow rate of CO2 gas introduced in the roller coating process is 2~4L / min, and the concentration is 80~100vol%; a 0.4~0.6mm thick coating is formed on the surface of the obtained enhanced bio-based lightweight aggregate.

2. The method for preparing the enhanced bio-based lightweight aggregate according to claim 1, characterized in that The sodium hydroxide solution in step 1 has a concentration of 0.01% to 0.07%, a pH value of 10 to 13, and a soaking time of 12 h to 24 h.

3. The method for preparing the enhanced bio-based lightweight aggregate according to claim 1, characterized in that The particle sizes after screening in step 2 are 5-20 mm and 0-5 mm respectively.

Citation Information

Patent Citations

  • Preparation method of novel core-shell type cement-based high-strength lightweight aggregate

    CN103496866A

  • Reinforced layer, reinforced lightweight aggregate and preparation method and application of reinforced lightweight aggregate

    CN114409292A

  • Method for preparing low-clinker cement slurry from commercial concrete wastewater by wet milling

    CN108298929A

  • Carbonization reinforced regenerated aggregate, and preparation method and applications thereof

    CN110357473A

  • Hollow recycled concrete component prepared by utilizing waste fiber and preparation method for hollow recycled concrete component

    CN110497517A