A method for preparing an integral nickel foam loaded NiCo2O4 nanosheet array
By performing solvent-thermal reaction and high-temperature calcining on nickel foam, an integral foam nickel-loaded NiCo2O4 nanosheet array was directly prepared, which solved the problems of complexity and high cost of nickel salt addition in the prior art, and achieved simplicity of operation and repeatability Good mass production.
Patent Information
- Application Number
- CN202310769157.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-28
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-06-28
AI Technical Summary
The existing solvent-thermal method requires additional nickel salt to be added, which is complex in operation, poor repetition and high cost, making it difficult to be suitable for large-scale production.
The monolithic nickel foam is used as the nickel source, and the solvent-thermal reaction is carried out by alcohol organic solvent and inorganic acid mixture, cobalt salt and hexamethylenetetramine to obtain the NiCo2O4 nanosheet precursor grown on the nickel foam, and at high temperature Calcination yields an integral foam nickel-supported NiCo2O4 nanosheet array, avoiding the additional nickel salt addition.
The preparation process is simplified, the cost is reduced, the morphological uniformity and mechanical stability of the product are improved, and it is suitable for large-scale production and provides a large number of active sites.
Smart Images

Figure CN116764638B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of inorganic nanomaterials, and in particular relates to a method for preparing an integral nickel foam loaded NiCo2O4 nanosheet array. Background Art
[0002] NiCo2O4 is a typical spinel-type mixed-valence metal composite oxide. In its crystal structure, nickel ions occupy octahedral positions, and cobalt ions occupy both octahedral and tetrahedral positions. NiCo2O4 is currently widely used in catalytic combustion of VOCs, fuel cells, air batteries, and supercapacitors.
[0003] The preparation method of NiCo2O4 nanomaterials has an important influence on their morphology and properties. Among them, the solvothermal method is a common method for preparing NiCo2O4. The NiCo2O4 nanomaterials prepared by the solvothermal method have the characteristics of high purity, good crystallinity and controllable morphology. At present, there are also studies that grow NiCo2O4 nanomaterials on the surface of a monolithic substrate (nickel foam, copper foam, etc.) to obtain NiCo2O4 nanoarrays with regular morphology (such as nanowires and nanosheets), which has attracted widespread attention from scientific researchers.
[0004] Currently, the solvothermal method for preparing NiCo2O4 nanoarrays usually requires the addition of nickel salts (such as nickel nitrate, nickel sulfate, etc.), which has problems such as complex operation, poor repeatability, and high cost. Therefore, it is necessary to develop a new method for preparing NiCo2O4 nanoarrays to further simplify the preparation process and reduce costs, making it more suitable for large-scale production. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the present invention provides a method for preparing an integral nickel foam loaded NiCo2O4 nanosheet array. The integral nickel foam loaded NiCo2O4 nanosheet array can be prepared by utilizing nickel foam to provide a nickel source without the need to add additional nickel salt. This method is simple to operate, has good repeatability, and the product morphology is uniform.
[0006] To achieve the above object, the present invention is implemented by the following technical solutions:
[0007] The first aspect of the present invention provides a method for preparing a monolithic nickel foam loaded NiCo2O4 nanosheet array, comprising the following steps:
[0008] S1, adding nickel foam to a mixture of an alcohol organic solvent and an inorganic acid, allowing it to stand, then adding cobalt salt and hexamethylenetetramine, and performing a solvothermal reaction after they are completely dissolved to obtain a NiCo2O4 nanosheet precursor grown on the nickel foam;
[0009] S2. Placing the precursor obtained in step S1 in an air atmosphere for high-temperature solid-phase reaction. After the reaction is complete, washing and drying are performed to obtain an integral nickel foam loaded NiCo2O4 nanosheet array.
[0010] The present invention uses nickel foam as a substrate, first dissolves part of the nickel foam by inorganic acid to replace the Ni 2+ , and then coprecipitated with cobalt salt and hexamethylenetetramine to in situ grow a two-dimensional sheet-like nanostructured nickel foam-loaded NiCo2O4 precursor on the nickel foam. The precursor was then placed in an air atmosphere for high-temperature calcination to finally obtain a nickel foam-loaded NiCo2O4 nanosheet array.
[0011] Preferably, in S1, the alcohol organic solvent includes methanol, and the inorganic acid includes concentrated nitric acid.
[0012] Preferably, in S1, the volume ratio of the inorganic acid to the alcohol organic solvent is 1:(300-500).
[0013] Preferably, in S1, the cobalt salt includes cobalt nitrate and cobalt sulfate.
[0014] Preferably, in S1, the molar ratio of the cobalt salt to hexamethylenetetramine is: 0.9-1.5:2.5-4.5.
[0015] Preferably, in S1, the ratio of the alcohol organic solvent to the cobalt salt is 30 mL: 0.9-1.5 mmol.
[0016] Preferably, in S1, the temperature of the thermal reaction is 100-140° C., and the time is 12-24 hours.
[0017] Preferably, in S2, the temperature of the high temperature solid phase reaction is 300-600°C, the time is 2-6h, and the heating rate is 1°C / min.
[0018] Preferably, the nickel foam is cleaned with acetone, hydrochloric acid, water and ethanol in sequence before use.
[0019] Preferably, the length×width×thickness of the nickel foam is cut to be 4×1×0.1 cm.
[0020] The second aspect of the present invention provides an integral nickel foam loaded NiCo2O4 nanosheet array prepared by the preparation method described in the first aspect.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The invention discloses a method for preparing a monolithic nickel foam loaded NiCo2O4 nanosheet array, wherein the nickel foam is first added to a mixed solution of an alcohol organic solvent and an inorganic acid, and then a cobalt salt and hexamethylenetetramine are added to perform a solvent thermal reaction to obtain a precursor, and then the precursor is subjected to high temperature roasting to obtain a monolithic nickel foam loaded NiCo2O4 nanosheet array. The method of the invention does not require the additional addition of nickel salts, and does not use a binder during the preparation process. The nickel foam is used as a direct nickel source and matrix, and a two-dimensional sheet-like nanostructure can be in-situ grown on the nickel foam through a solvent thermal reaction and a high-temperature solid phase reaction, which not only enhances the mechanical stability of the monolithic material, but also provides a large number of effective active sites. At the same time, the method of the invention is simple and easy to operate, convenient to control, good in repeatability, low in cost, and suitable for large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is the X-ray powder diffraction pattern of the monolithic nickel foam loaded NiCo2O4 nanosheet array in Example 1;
[0024] Figure 2 This is a scanning electron microscope image of the monolithic nickel foam loaded NiCo2O4 nanosheet array in Example 1;
[0025] Figure 3 This is the EDS spectrum of the monolithic nickel foam loaded NiCo2O4 nanosheet array in Example 1;
[0026] Figure 4 This is the X-ray powder diffraction pattern of the monolithic nickel foam loaded with Co3O4 in Comparative Example 1;
[0027] Figure 5 This is a scanning electron microscope image of the monolithic nickel foam loaded with Co3O4 in Comparative Example 1;
[0028] Figure 6 This is the EDS energy spectrum of the integral nickel foam loaded with Co3O4 in Comparative Example 1. DETAILED DESCRIPTION
[0029] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0030] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0031] Example 1 Preparation method of a monolithic nickel foam loaded NiCo2O4 nanosheet array
[0032] The specific preparation method comprises the following steps:
[0033] (1) A nickel foam having a length×width×thickness of 4×1×0.1 cm was ultrasonically cleaned in acetone, 0.2 mol / L hydrochloric acid, ultrapure water, and anhydrous ethanol for 5 min in sequence, and then placed in a vacuum oven and vacuum dried at 60°C for 12 h before use.
[0034] (2) Place clean nickel foam vertically into a reaction kettle, and then pour 0.06mL of a mixture of 68% concentrated nitric acid and 30mL of methanol into the kettle and let it stand for 0.5h. Then add 0.90mmol of Co(NO3)2·6H2O and 2.50mmol of hexamethylenetetramine into the kettle and dissolve them completely, and react at 100℃ for 24h. Then wash and dry the product to obtain a monolithic nickel foam loaded NiCo2O4 nanosheet array precursor.
[0035] (3) The precursor is placed in a muffle furnace for high-temperature calcination, and the temperature is increased to 300°C at a heating rate of 1°C / min, and maintained in an air atmosphere for 6 hours. After the reaction is completed, it is cooled to room temperature, and the obtained product is washed alternately with deionized water and anhydrous ethanol three times in sequence, and finally the product is dried in an oven to obtain a monolithic nickel foam loaded NiCo2O4 nanosheet array.
[0036] The nickel foam loaded NiCo2O4 nanosheets obtained above were tested and characterized. The results of X-ray powder diffraction are as follows Figure 1 As shown in the figure, it can be seen that the prepared product corresponds to NiCo2O4 indicated by JCPDF standard card #20-0781, and there are no other impurity peaks, indicating that pure NiCo2O4 has been synthesized. The results of the scanning electron microscope are shown in Figure 2 As shown in the figure, it can be seen that its morphology is uniform and has a nanosheet structure. Its EDS spectrum is as follows Figure 3 As shown, it can be seen from the figure that the mass content percentage of nickel in NiCo2O4 is 23.06%.
[0037] Example 2 Preparation method of a monolithic nickel foam loaded NiCo2O4 nanosheet array
[0038] The specific preparation method comprises the following steps:
[0039] (1) A nickel foam having a length×width×thickness of 4×1×0.1 cm was ultrasonically cleaned in acetone, 0.2 mol / L hydrochloric acid, ultrapure water, and anhydrous ethanol for 5 min in sequence, and then placed in a vacuum oven and vacuum dried at 60°C for 12 h before use.
[0040] (2) Place clean nickel foam vertically into a reaction kettle, and then pour 0.1 mL of a mixture of 68% concentrated nitric acid and 30 mL of methanol into the kettle and let it stand for 0.5 h. Then add 1.50 mmol of Co(NO3)2·6H2O and 4.50 mmol of hexamethylenetetramine into the kettle and dissolve them completely, and react at 140°C for 12 h. Then wash and dry the product to obtain a monolithic nickel foam loaded NiCo2O4 nanosheet array precursor.
[0041] (3) The precursor is placed in a muffle furnace for high-temperature calcination, and the temperature is increased to 600°C at a heating rate of 1°C / min, and maintained in an air atmosphere for 6 hours. After the reaction is completed, it is cooled to room temperature, and the obtained product is washed alternately with deionized water and anhydrous ethanol for three times, and finally the product is dried in an oven to obtain a monolithic nickel foam loaded NiCo2O4 nanosheet array.
[0042] Consistent with Example 1, pure phase NiCo2O4 was successfully synthesized with uniform morphology and nanosheet structure, and the mass content percentage of nickel was 23.49%.
[0043] Comparative Example 1 Preparation method of a monolithic nickel foam loaded Co3O4 nanosheet array
[0044] The specific preparation method is generally the same as that of Example 1, except that: Step (2) is specifically as follows: Place clean nickel foam vertically into a reaction kettle, then pour 30 mL of a methanol mixture into the kettle and let stand for 0.5 h. Then add 0.90 mmol of Co(NO3)2·6H2O and 2.50 mmol of hexamethylenetetramine into the kettle and dissolve completely, and react at 100°C for 24 h, then wash and dry the product to obtain a monolithic nickel foam loaded NiCo2O4 nanosheet array precursor.
[0045] The above product was tested and characterized. The results of its X-ray powder diffraction are as follows Figure 4 As shown in the figure, it can be seen that the prepared product corresponds to Co3O4 indicated by JCPDF standard card #09-0418, and there are no other impurity peaks, indicating that pure phase Co3O4 has been synthesized. The results of the scanning electron microscope are shown in Figure 5 As shown in the figure, it can be seen that its morphology is a uniform array of nanosheets. Its EDS spectrum is as follows Figure 6 As shown in the figure, it can be seen that there is no nickel in the Co3O4. However, compared with Example 1, without adding acid corrosion, it is impossible to generate a monolithic nickel foam loaded NiCo2O4 nanosheet array.
[0046] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for preparing a monolithic nickel foam loaded NiCo2O4 nanosheet array, characterized in that: The following steps are involved: S1. Adding nickel foam to a mixed solution of an alcohol organic solvent and an inorganic acid, wherein the alcohol organic solvent includes methanol, the inorganic acid includes concentrated nitric acid, and the volume ratio of the inorganic acid to the alcohol organic solvent is 1:(300-500). After standing, cobalt salt and hexamethylenetetramine are added, wherein the molar ratio of the cobalt salt to hexamethylenetetramine is 0.9-1.5:2.5-4.5, and the amount ratio of the alcohol organic solvent to the cobalt salt is 30mL:0.9-1.5mmol. After complete dissolution, a solvent thermal reaction is performed at a temperature of 100-140°C for 12-24h to obtain a NiCo2O4 nanosheet precursor grown on nickel foam; S2. Place the precursor obtained in step S1 in an air atmosphere for a high-temperature solid-phase reaction at a temperature of 300-600°C for 2-6 hours at a heating rate of 1°C / min. After the reaction is complete, a more regular and uniform integral nickel foam-loaded NiCo2O4 nanosheet array can be obtained by washing and drying.
2. The method for preparing a monolithic nickel foam loaded NiCo2O4 nanosheet array according to claim 1, characterized in that: In S1, the cobalt salt includes cobalt nitrate and cobalt sulfate.
3. The method for preparing a monolithic nickel foam loaded NiCo2O4 nanosheet array according to claim 1, characterized in that: The nickel foam is cleaned with acetone, hydrochloric acid, water and ethanol in sequence before use.
4. An integral nickel foam loaded NiCo2O4 nanosheet array prepared by the preparation method according to any one of claims 1 to 3.