Carbon dioxide adduct foaming agent containing aromatic ring polyamine polymer and its application

Polyamine polymers containing aromatic rings are generated through the reaction of aromatic dialdehydes and aliphatic polyamines, which are used to prepare CO2 adduct foaming agents. This solves the problems of poor dispersion and high cost of PEI-CO2 adducts and achieves Good dispersion in polyurethane raw materials and excellent compatibility in bio-based polyols are suitable for industrial applications.

CN116790020BActive Publication Date: 2024-10-29SICHUAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310749550.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-21
Publication Date
2024-10-29
Estimated Expiration
2043-06-21

AI Technical Summary

Technical Problem

The existing PEI-CO2 adduct foaming agent has poor dispersion in polyurethane foam materials, and due to the high price of PEI, it is difficult to apply industrially. Traditional fluorine- and chlorine-containing foaming agents are harmful to the environment.

Method used

Aromatic dialdehydes are reacted with aliphatic polyamines to generate Schiff base-containing polyamine polymers, and the aromatic ring-containing polyamine polymers are obtained through hydrogenation and reduction, which are used to react with CO2 to generate new CO2 adduct foaming agents. , improve its dispersion performance and cost-effectiveness in polyurethane raw materials.

Benefits of technology

It achieves good dispersion in polyurethane raw materials and excellent compatibility in bio-based polyols, reduces the production cost of foaming agents, is suitable for industrial applications, and maintains good redispersibility after long-term storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116790020B_ABST
    Figure CN116790020B_ABST
Patent Text Reader

Abstract

The invention discloses a graft-modified polyamine polymer having an aromatic ring in the main chain. 2 Adduct foaming agent, the main chain of the polyamine polymer is prepared by aldehyde-amine condensation of aliphatic polyamine compounds and aromatic dialdehydes and reduction of the resulting Schiff base. The aliphatic polyamine compound contains at least two primary amines, including a diprimary amine with a carbon number not greater than 6, and polyethyleneimine, polypropyleneimine or polybutyleneimine with a degree of polymerization of 2 to 20; the aromatic ring of the aromatic dialdehyde includes at least one of benzene, biphenyl, furan, thiophene, pyridine, pyrimidine, bipyridine, carbazole, diphenyl ether, naphthalene, anthracene, phenanthrene, pyrene, pyrazine, pyrrole and indole. The polyamine polymer is grafted with side chains such as alkyl chains and polypropylene oxide. The aromatic ring-containing CO 2 The adduct foaming agent has good dispersibility in vegetable oil-based polyols and can be redispersed by stirring even if it precipitates from the system, so it is suitable for preparing bio-based polyurethane foams.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of foaming agents and their preparation and application, and specifically relates to the preparation of an aromatic ring-containing polyamine polymer foaming agent capable of releasing carbon dioxide (CO2) and the application of the foaming agent in polyurethane foam materials. Background Art

[0002] The global annual production of polyurethane (PU) has exceeded 22 million tons, of which 65% of the market share comes from PU foam, the manufacture of which requires a large amount of auxiliary foaming agents. Traditional fluorine-containing and chlorine-containing foaming agents will aggravate global warming and more or less damage the ozone layer in the stratosphere. Recently, researchers have developed a series of CO2 adducts of hydrophobically modified polyethyleneimine (PEI) and used them as PU foaming agents, which are environmentally friendly foaming agents. If PEI is not modified, the zwitterions (carbamate anions and alkyl ammonium cations) in the PEI-CO2 adduct have high hydrophilicity, making the PEI-CO2 adduct difficult to disperse. Hydrophobic modification is conducive to the dispersion of PEI's CO2 adduct into hydrophobic PU raw materials. In order to further obtain good dispersibility, it is usually necessary to add small molecule flame retardants as diluents to the foaming system. Without using a diluent, the researchers completely mixed hydrophobically modified PEI and polyether polyol (both in liquid form) to absorb CO2, in situ forming PEI-CO2 adduct nanoparticles suspended in the polyether polyol. Even though the foaming mixture obtained by this method showed a higher viscosity than the original mixture without CO2 absorption, it can also be used to prepare PU foams.

[0003] Since the CO2 adduct foaming agent based on PEI is solid, it is naturally difficult to disperse into the PU raw material. The dispersibility can be appropriately improved by grafting modification of PEI, introducing small molecule flame retardants into the formula, and preparing the foaming agent in situ in polyether. In addition, due to the high price of PEI, it is difficult to industrialize the CO2 adduct foaming agent based on PEI. The main reason for the high price of PEI is that the monomer aziridine of PEI is highly toxic, and it needs to be carefully stored and transported to prevent any leakage, and the equipment and management costs are high.

[0004] PEI oligomers (including ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, etc.), due to their polyamine structure, can also absorb CO2 to form CO2 adducts. Such compounds are prepared by reacting ethylene dichloride with water and ammonia at high temperature (120-180°C) and high pressure (2.0-2.5MPa), and are relatively cheap. Like PEI, PEI oligomers can also react with CO2 to form adducts. However, the molecular chain of PEI oligomers is relatively short, and it is difficult to graft hydrophobic chains for modification, which hinders the application of CO2 adducts of PEI oligomers as PU foaming agents. Summary of the invention

[0005] In view of the shortcomings of the prior art, the inventors explored the preparation of polyamine polymers by dialdehyde chain extension reaction of aliphatic polyamine compounds. If the dialdehyde is an aliphatic dialdehyde, such as glyoxal, malondialdehyde, etc., it is easy to obtain a cyclic compound. At the same time, the Schiff base (-C=N-) generated by aliphatic amines and aliphatic aldehydes is unstable, and it is difficult to obtain a polyamine polymer with a high molecular weight. To this end, we use aromatic dialdehydes and aliphatic polyamines to react to obtain a polymer containing a Schiff base, and obtain a polyamine polymer containing an aromatic ring by hydrogenating and reducing the Schiff base. The polyamine polymer can react with CO2 to generate a new type of CO2 adduct for PU foaming. This foaming agent is cheaper than the foaming agent prepared by PEI. During the research process, the inventors unexpectedly found that the introduction of aromatic rings makes the foaming agent have better dispersibility in bio-based polyols, and it can be redispersed after long-term storage, which is very important for industrial applications.

[0006] One of the purposes of the present invention is to provide a CO2 adduct foaming agent of a grafted modified polyamine polymer containing an aromatic ring. The CO2 adduct consists of a grafted polyamine polymer and CO2, wherein the grafted polyamine polymer and CO2 form an adduct, and the main chain structure of the grafted polyamine polymer is:

[0007]

[0008] Wherein, R1 is a structure obtained by removing the terminal primary amine group from an aliphatic polyamine compound, wherein the aliphatic polyamine compound contains at least two primary amines, including but not limited to a dibasic primary amine having a carbon number not greater than 6, and polyethyleneimine, polypropyleneimine or polybutyleneimine having a degree of polymerization of 2 to 20; R2 is a structure obtained by removing the aldehyde group from an aromatic dialdehyde, wherein the aromatic ring of the aromatic dialdehyde includes but is not limited to benzene, biphenyl, furan, thiophene, pyridine, pyrimidine, bipyridine, carbazole, diphenyl ether, naphthalene, anthracene, phenanthrene, pyrene, pyrazine, pyrrole and indole; n is an integer not less than 1; and the terminal group of the polyamine polymer is at least one of an amine group and a hydroxyl group;

[0009] The side chains of the grafted polyamine polymer include but are not limited to at least one of the following:

[0010] (1) The side chain is polyethylene glycol, polypropylene oxide, polyoxetane, polytetrahydrofuran or polysiloxane, and the degree of polymerization is at least 1;

[0011] (2) The side chain contains a trimethylsilyl group;

[0012] (3) The side chain contains a hydrocarbon group having 1 to 22 carbon atoms;

[0013] (4) The side chain contains a fluorinated alkyl group having 1 to 22 carbon atoms;

[0014] The grafting rate of the grafted polyamine polymer is 0 to 45 mol % based on the N atoms in the main chain of the polyamine polymer.

[0015] The main chain of the above-mentioned polyamine polymer can be prepared by reacting aliphatic polyamine compounds and aromatic dialdehydes. The primary amines of the aliphatic polyamine compounds and aldehydes are condensed to form Schiff bases, and the Schiff bases are reduced by hydrogenation to obtain polyamine polymers containing aromatic rings. The aliphatic polyamine compound contains at least two primary amines, including but not limited to dibasic primary amines with a carbon number not greater than 6, and polyethyleneimine, polypropyleneimine or polybutyleneimine with a degree of polymerization of 2 to 20; the aromatic ring of the aromatic dialdehyde includes but is not limited to at least one of benzene, biphenyl, furan, thiophene, pyridine, pyrimidine, bipyridine, carbazole, diphenyl ether, naphthalene, anthracene, phenanthrene, pyrene, pyrazine, pyrrole and indole. Usually, in order to increase the amino content of the prepared polyamine polymer, the molar ratio of the aliphatic polyamine compound and the aromatic dialdehyde is greater than 1, and the terminal group of the obtained polymer is an amino group; of course, the molar ratio can also be less than 1, and the terminal group of the obtained polymer is an aldehyde group, and the terminal group of the polyamine polymer obtained after reduction is a hydroxyl group.

[0016] It should be pointed out that it is not feasible to use aliphatic dialdehydes to replace the aromatic dialdehydes of the present invention. The Schiff base (-C=N-) generated by the aromatic dialdehyde and the aliphatic polyamine compound can be stabilized by conjugation with the aromatic ring, and a polyamine polymer containing an aromatic ring can be obtained by selective hydrogenation. The Schiff base generated by the aliphatic dialdehyde has no conjugation effect, is unstable, and will degrade, making it difficult to obtain a high molecular weight polymer.

[0017] In order to give the prepared polyamine polymer certain flame retardant properties (it can act as a foaming agent and flame retardant), the aromatic dialdehyde may contain halogen substituents, such as chlorine or bromine substituents, in addition to two aldehyde substituents. Some aromatic dialdehydes also carry alkyl substituents, which can give the prepared polyamine polymer a certain hydrophobicity, which is conducive to the dispersion of the final CO2 adduct foaming agent of the polyamine polymer into the raw materials of the polyurethane, so as to better play the role of foaming. The number of carbon atoms of the alkyl group is 1 to 22. An example of an aromatic dialdehyde with an alkyl chain is 9-(2-ethylhexyl)carbazole-3,6-dicarboxaldehyde, whose structure is:

[0018]

[0019] Since the structure of aromatic dialdehydes does not absorb CO2, the aromatic ring of the aromatic dialdehyde should be as small as possible, so that the proportion of amino groups in the synthesized polyamine polymer is higher, and the CO2 content of the prepared foaming agent will be higher. The aromatic ring is preferably at least one of benzene, pyridine, biphenyl, furan, naphthalene, and anthracene. Further, the aromatic ring is preferably benzene.

[0020] In order to make the final polyamine polymer have a high amine content, the amine content of the aliphatic polyamine compound should be as high as possible, and polyethyleneimine is a commercially available polymer with the highest amine content. In the present invention, the raw material aliphatic polyamine compound of the polyamine polymer is preferably polyethyleneimine oligomer, with a degree of polymerization between 2 and 10, and can be a linear or branched polymer, and can also contain a piperazine ring; preferably a linear polyethyleneimine oligomer, such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, hexaethyleneheptamine, heptaethyleneoctamine, octaethylenenonamine, nonaethylenedecaamine, and decaethyleneundecamine.

[0021] In the present invention, the polyamine polymer is prepared by the following process steps:

[0022] (1) dissolving 1 mol of an aromatic dialdehyde in methanol or ethanol, adding 0.5 to 2 mol of an aliphatic polyamine compound, and reacting at 60 to 80° C. for 8 to 24 hours; after cooling to room temperature, adding a reducing agent, and reacting at room temperature for 12 to 36 hours; the reducing agent may be at least one of sodium borohydride or hydrogen;

[0023] (2) The mixture obtained in step (1) is subjected to the steps of desalting (or filtering), desolventizing, and vacuum drying to obtain a transparent viscous liquid product, which is a polyamine polymer containing an aromatic ring.

[0024] Furthermore, the molar fraction of the aliphatic polyamine compound in the above process step (1) is 1.02 to 1.1.

[0025] Furthermore, the aliphatic polyamine compound in the above process step (1) is tetraethylenepentamine or pentaethylenehexamine.

[0026] Furthermore, the reducing agent in the above process step (1) can be at least one of sodium borohydride or hydrogen. Sodium borohydride can be used for small-scale laboratory production, and catalytic hydrogenation can be used for industrial production. The reducing agent selectively reduces the Schiff base without reducing the aromatic ring. Those skilled in the art can select a suitable reduction method as needed.

[0027] After preparing the above-mentioned polyamine polymer containing aromatic rings, side chains can be further grafted onto the main chain of the polyamine polymer. The foaming agent obtained after the grafting of side chains has better dispersibility in polyurethane raw materials, especially it is easy to disperse in vegetable oil polyols. The side chains include but are not limited to at least one of the following:

[0028] (1) The side chain is polyethylene glycol, polypropylene oxide, polyoxetane, polytetrahydrofuran or polysiloxane, and the degree of polymerization is at least 1;

[0029] (2) The side chain contains a trimethylsilyl group;

[0030] (3) The side chain contains a hydrocarbon group having 1 to 22 carbon atoms;

[0031] (4) The side chain contains a fluorinated alkyl group having 1 to 22 carbon atoms.

[0032] Specifically, the grafted side chain can be a polyether oligomer such as polyethylene glycol, polypropylene oxide, polyoxetane and polytetrahydrofuran, or polysiloxane, containing at least one repeating unit, and the structure is exemplified as follows:

[0033]

[0034] Wherein m is at least 1, n is a positive integer from 1 to 4, and Q and T are connecting groups between the grafted side chain and the main chain of the polyamine polymer. The connecting groups Q and T are replaceable groups, and the groups that can be selected are:

[0035]

[0036]

[0037] The grafted side chain of the grafted polyamine polymer may also contain silane, and its structure may be:

[0038]

[0039] T is a linking group between the side chain and the main chain of the polyamine polymer, and T can be:

[0040]

[0041] The grafted side chain of the grafted polyamine polymer may also contain a hydrocarbon group with 1 to 22 carbon atoms and at least one unsaturated bond, and its structure is exemplified as follows:

[0042] C n H 2n-1 -M-,

[0043] Wherein n is an integer from 1 to 22, and M is a linking group between the hydrophobic side chain and the main chain of the polyamine polymer. The linking group M is a replaceable group, and M can be directly a covalent bond or an amide bond.

[0044] The grafted side chain of the grafted polyamine polymer may also contain an alkyl group or a fluorinated alkyl group having 1 to 22 carbon atoms, and its structure is exemplified as follows:

[0045] C n H 2n+1-m F m -M-,

[0046] Wherein n is an integer from 1 to 22, m is an integer from 0 or 1 to 43, and M is a linking group between the grafted side chain and the main chain of the polyamine polymer. The linking group M is a replaceable group, and M can be directly a covalent bond or an amide bond, and can also be selected from the following groups:

[0047]

[0048] It should be pointed out that the linking groups Q, T and M between the above-mentioned grafted side chains and the main chain of the polyamine polymer are all replaceable groups, and those skilled in the art can also select other groups for replacement, which are not listed here one by one.

[0049] As for the specific preparation method of the above-mentioned grafted polyamine polymer, the glycidyl ether with grafted side chains and the polyamine polymer can be reacted in an ethanol solution to obtain a grafted modified polyamine polymer. The structure of the glycidyl ether with a hydrophobic chain is:

[0050]

[0051] wherein m is at least 1, and n is a positive integer from 1 to 4. The linking group between the side chain and the main chain of the grafted polyamine polymer prepared by this method is Q1; the structure of the glycidyl ether with a hydrophobic chain can also be:

[0052]

[0053] Wherein m is 0 or a positive integer, and the linking group between the side chain and the main chain of the grafted polyamine polymer prepared by this method is T; the structure of the glycidyl ether with a hydrophobic chain can also be:

[0054]

[0055] Wherein n is an integer from 1 to 22, m is an integer from 0 or 1 to 43, and the linking group between the side chain and the main chain of the grafted polyamine polymer prepared by this method is M2.

[0056] Alternatively, an alkyl group with an epoxy group or a fluorinated alkyl group with an epoxy group and a polyamine polymer may be reacted in an ethanol solution to obtain a grafted polyamine polymer. The structure of the alkyl group with an epoxy group or the fluorinated alkyl group may be:

[0057]

[0058] Wherein n is an integer from 1 to 22, m is an integer from 0 or 1 to 43, and the linking group between the side chain and the main chain of the grafted polyamine polymer prepared by this method is M1.

[0059] The grafted polyamine polymer can also be prepared by the following method: first, the alkoxy polyether oligomer is reacted with iodoacetic acid and 2-bromoisocyanate to obtain a halogenated hydrocarbon-terminated product, and the reaction is as follows (wherein m is at least 1, and n is a positive integer from 1 to 4):

[0060]

[0061] The above reaction is based on an alkoxy polypropylene glycol oligomer as an example, wherein the repeating units may also be repeating units of polyethylene glycol, polyoxetane and polytetrahydrofuran.

[0062] Secondly, the above-mentioned halogenated hydrocarbon end-capping product is reacted with a polyamine polymer to remove hydrogen halide to obtain an N-substituted hydrophobically modified polyamine polymer (the linking group between the side chain and the main chain is Q2 or Q3).

[0063] The grafted polyamine polymer can also be prepared by reacting a bromide or iodide of an alkane or a fluorine-containing alkane with a polyamine polymer. The structure of the bromide or iodide can be:

[0064] C n H 2n+1-m F m -Br, or C n H 2n+1-m F m -I,

[0065] wherein n is an integer from 1 to 22, and m is an integer from 0 or 1 to 43. The linking group between the side chain and the main chain of the grafted polyamine polymer prepared by this method is a covalent bond.

[0066] The grafted polyamine polymer can also be prepared by reacting an alkyl or fluorinated alkyl carboxylic acid with a polyamine polymer. The structure of the carboxylic acid can be:

[0067] C n H 2n+1-m F m -COOH,

[0068] wherein n is an integer from 1 to 22, and m is an integer from 0 or 1 to 43. The linking group between the side chain and the main chain of the grafted polyamine polymer prepared by this method is an amide bond.

[0069] The grafted polyamine polymer can also be prepared by reacting unsaturated fatty acids with polyamine polymers. The structure of the fatty acid can be:

[0070] C n H 2n-1 -M-,

[0071] wherein n is an integer from 1 to 22. The linking group M between the side chain and the main chain of the grafted polyamine polymer prepared by this method is an amide bond.

[0072] All these reactions are known chemical reactions, and their specific preparation methods can refer to existing disclosed technologies, such as patent document CN 108355472 A.

[0073] In addition, in the preparation method of the grafted polyamine polymer provided by the present invention, the grafting degree of the grafted polyamine polymer is 0 to 45 mol% based on the N atoms of the polyamine polymer. Preferably, the grafting degree of the grafted polyamine polymer is 3 to 20 mol% based on the N atoms of the polyamine polymer. Generally, the greater the grafting degree of the grafted polyamine polymer, the more conducive it is to its dispersion in the polyurethane raw material. However, if the grafting rate is too large, the proportion of amino groups that react with CO2 in the grafted polyamine polymer will decrease, and the CO2 content in the grafted polyamine polymer CO2 adduct will decrease, thereby reducing the foaming ability.

[0074] The polyamine polymer provided by the present invention has an aromatic ring, which increases the hydrophobicity of the polyamine polymer and is conducive to the reaction with CO2; at the same time, the obtained CO2 adduct foaming agent of the polyamine polymer has an aromatic ring in the main chain, which weakens the intermolecular force of the zwitterions (carbamate anions and alkyl ammonium cations) in the CO2 adduct, so that the obtained CO2 adduct foaming agent is more easily dispersed in polyurethane raw materials, especially in vegetable oil polyols. The preparation method of the CO2 adduct foaming agent of the grafted polyamine polymer is as follows: take 1 mass part of the polyamine polymer and dissolve it in ethanol to obtain a polyamine polymer solution with a mass concentration of 10-50%, put it into a closed reactor, pass 0.1-1MPa CO2 to react for 1-3 hours, obtain a white precipitate, filter to remove the solvent, then vacuum dry at 40°C for 1-3 days, then put it into a closed reactor and pass 0.5MPa CO2 to maintain pressure for 2 days to obtain the CO2 adduct foaming agent of the polyamine polymer.

[0075] Another object of the present invention is to provide the grafted polyamine polymer CO2 adduct foaming agent for use in preparing polyurethane foam. The grafted polyamine polymer CO2 adduct foaming agent contains an aromatic ring, which weakens the intermolecular force of zwitterions (carbamate anions and alkyl ammonium cations) in the CO2 adduct, making the obtained CO2 adduct foaming agent easier to disperse into polyurethane raw materials. The white material containing the foaming agent (the components of the polyurethane foam raw materials other than isocyanate are white materials; isocyanate is black material) can be stored for a long time, and even if stratification occurs, it is easy to disperse it into the white material by stirring.

[0076] Another object of the present invention is to provide the CO2 adduct blowing agent of the grafted polyamine polymer for use in preparing bio-based polyol polyurethane foam. The CO2 adduct blowing agent of the grafted polyamine polymer is particularly easy to disperse in bio-based polyol (such as castor oil-based polyol) and is particularly suitable for preparing bio-based polyol polyurethane foam.

[0077] Compared with the prior art, the present invention has the following positive effects:

[0078] 1. The present invention uses aromatic dialdehyde as raw material, reacts with aliphatic polyamine compounds to generate Schiff base, and then reduces to obtain polyamine polymers containing aromatic rings in the molecule, thereby avoiding the use of toxic aziridine to prepare polyamine polymers.

[0079] 2. The aromatic ring-containing polyamine polymer prepared by the present invention uses cheap and readily available raw materials, has little pollution, is simple to operate, and is easy to promote industrialization.

[0080] 3. The polyamine polymer containing aromatic rings prepared by the present invention has a benzene ring in the molecule, so the compatibility of the CO2 adduct foaming agent prepared with it as a raw material in polyurethane raw materials is better than that of the polyamine polymer without aromatic rings. In particular, it has good compatibility in vegetable oil polyols and is suitable for preparing bio-based polyurethane foams. BRIEF DESCRIPTION OF THE DRAWINGS

[0081] Attached Figure 1 The structures and codes of the aromatic dialdehydes used in the raw material preparation examples (1) to (20) are shown below.

[0082] Attached Figure 2 The chemical structures of the phenyl ring-containing polyamine polymers prepared in Examples (1) to (4) are shown in the attached table. Figure 3 and 4 NMR spectrum.

[0083] Attached Figure 3 This is the H NMR spectrum of the benzene ring-containing polyamine polymer (xPEIP, x represents the molecular weight) prepared in the raw material preparation examples (1) to (4). The spectra from top to bottom are from the products of the raw material preparation examples (4), (3), (2) and (1).

[0084] Attached Figure 4 The NMR carbon spectra of the polyamine polymers containing benzene rings (xPEIP, x represents the molecular weight) prepared from the raw material examples (1) to (4). The spectra from top to bottom are from the products of examples (4), (3), (2) and (1).

[0085] Attached Figure 5 The chemical structural formulas and codes of the side chain raw materials used in preparing the grafted polyamine polymers in Examples 21 to 47.

[0086] Attached Figure 6 This is the infrared spectrum of the CO2 adduct of the benzene ring-containing polyamine polymer prepared in Examples 2 and 21-26.

[0087] Attached Figure 7 The compatibility of different CO2 adduct foaming agents in castor oil-based polyol Polycin M-365 is observed. The blank is pure Polycin M-365, and the other samples contain 2% mass concentration of foaming agent. In the left group of samples, 10% C8-PEI-CO2 is a CO2 adduct foaming agent formed by branched polyethyleneimine (molecular weight 2500) grafted with 10% octyl side chains, and the foaming agents of x=1.8k, 3.6k, 9.1k and 17.8k are from Examples 21 to 24 respectively; in the right group of samples, 3.6kPEIP-CO2 is from Example 2, and y=5%, 10% and 15% of the foaming agents are from Examples 25, 22 and 24 respectively. In the figure, * indicates that the foaming mixture is translucent and has no precipitation; # indicates that precipitation has occurred in the foaming mixture; the white arrow indicates that the dent in the corner behind the sample can be clearly seen, indicating that the foaming mixture is in a uniform and transparent state.

[0088] Attached Figure 8 The compatibility of different CO2 adduct foaming agents in polyether 4110 is observed. The blank is pure polyether 4110, and the other samples contain 2% mass concentration of foaming agent. 10% C8-PEI-CO2 is a CO2 adduct foaming agent formed by branched polyethyleneimine (molecular weight 2500) grafted with 10% octyl side chains; 3.6kPEIP-CO2 comes from Example 2; y=5%, 10% and 15% of the foaming agent come from Application Examples 29, 30 and 31 respectively. The arrows indicate that the foaming mixture has precipitated. DETAILED DESCRIPTION

[0089] In order to make the purpose, technical scheme and technical effect of the present invention clearer, the present invention is further described in detail in conjunction with specific embodiments below. It should be noted that all these embodiments are for further illustrating the present invention and shall not be construed as limiting the present invention. Some non-essential improvements and adjustments made by those skilled in the art to the present invention according to the above-mentioned content of the present invention still belong to the protection scope of the present invention.

[0090] Raw material preparation examples (1) to (20)

[0091] This group of raw material preparation examples prepares polyamine polymers containing aromatic rings as raw materials. The aliphatic polyamine compound used contains at least two primary amines, which can be selected from dibasic primary amines with a carbon number not greater than 6, and polyethylene imine (PEI), polypropylene imine (PPI) or polybutylene imine (PBI) with a degree of polymerization of 2 to 20. Specifically, the aliphatic polyamines selected in this group of examples are: 1,2-ethylenediamine (EDA), 1,4-butylene diamine (BDA), 1,6-hexanediamine (HDA), diethylenetriamine (PEI2), triethylenetetramine (PEI3), tetraethylenepentamine (PEI4), pentaethylenehexamine (PEI5), linear PEI-430 (molecular weight 430, degree of polymerization of about 10), branched PEI-860 (molecular weight 860, degree of polymerization of about 20), polypropylene imine pentamer (PPI5), polybutylene imine octamer (PBI8).

[0092] Table 1

[0093]

[0094] The aromatic ring of the aromatic dialdehyde used can be selected from benzene, biphenyl, furan, thiophene, pyridine, pyrimidine, bipyridine, carbazole, diphenyl ether, naphthalene, anthracene, phenanthrene, pyrene, pyrazine, pyrrole, and indole, and the aromatic ring can be substituted with halogen or alkyl chain. Specifically, the aromatic dialdehydes selected in this group of embodiments include terephthalaldehyde (TPA), o-phthalaldehyde (OPA), 2,3-naphthalene dicarboxaldehyde (NDA), 9,10-anthracene dicarboxaldehyde (ADA), 4,4′-biphenyl dicarboxaldehyde (BpDA), 2,5-furan dicarboxaldehyde (FuDA), 2,6-pyridine dicarboxaldehyde (PyDA), 3,4-dibromothiophene-2,5-dicarboxaldehyde (BrTDA), 5-fluoro-2,3-thiophene dicarboxaldehyde (FTDA), 2,2′-bipyridine-4,4′-dicarboxaldehyde (BPyDA), 9-(2-ethylhexyl)carbazole-3,6-dicarboxaldehyde (C8-CzDA), and 4-(4-formylphenoxy)benzaldehyde (MpBA). The structures and codes of the selected dialdehydes are shown in Figure 1 .

[0095] Table 1 lists the raw materials used in the preparation examples (1) to (20) of the polyamine polymers and the molecular weight and structure of the obtained aromatic ring-containing polyamine polymers. The code of each raw material is as described above. When mixed polyamines or dialdehydes are used, the molar proportion of each raw material is also listed (the total molar amount is 1). The raw material ratio refers to the molar ratio of polyamine to dialdehyde. In the table, n is the number of repeating units calculated based on the raw material ratio.

[0096] The preparation process of the polyamine polymer containing aromatic rings in Table 1 is as follows: 1 mol of aromatic dialdehyde is added to ethanol to make the mass concentration 10%, and then the corresponding aliphatic polyamine is added according to the raw material ratio in Table 1. The reaction temperature is raised, refluxed for 12 hours, and then naturally lowered to room temperature. Then 4 mol of sodium borohydride is added, 0.4 mol is added every 20 minutes, and after the addition is completed, it is stirred at room temperature for 12 hours, and 2 mol of water is added to quench the reaction, and the salt is dialyzed with a dialysis bag with a molecular weight cutoff of 100 to remove the salt, and the dialyzate is concentrated and dried to obtain a viscous oily product.

[0097] Figure 2 This is a schematic diagram of the structure of the products obtained from Examples (1) to (4) of the raw materials. This group of products contains a benzene ring and is represented by xPEIP (x is the actual molecular weight, in kDa, see Table 1). Figure 3 The H NMR spectra of xPEIP and raw material PEI5 were compared. All samples had N–CH2 signals in the range of 2.4 to 2.8 ppm, while the product xPEIP showed C–H of the benzene ring and CH2 signals near the benzene ring at 7.23 ppm (k peak) and 3.63 ppm (l peak). Figure 4 The NMR carbon spectra of xPEIP and raw material PEI5 were compared. PEI5 showed three main carbon peaks (C12, C22 and C21) at 39.84, 47.67 and 50.70 ppm. Among these three signals, xPEIP only retained the carbon signal related to the secondary amine (C22). In addition, the signals from carbons in and near the benzene ring (peaks p, k and l at 138.02, 128.72 and 52.12 ppm, respectively) were consistent with expectations. The NMR spectrum clearly shows that the condensation between PEI5 and TPA occurs on the primary amine group at the end of PEI5, and the formed Schiff base (–C=N–) is completely reduced to a secondary amine (because the corresponding signal of the Schiff base was not observed). Figure 3 In the above, the molar ratio of PEI5 to TPA chain segments can be obtained by the area ratio of the proton signal peak (N–CH2) corresponding to the PEI5 chain segment and the proton signal peak (k) corresponding to the benzene ring, thereby calculating the actual number average molecular weight of the sample (represented by x), which is the actual molecular weight listed in Table 1. The other products in Table 1 can also be measured by nuclear magnetic hydrogen spectrum (dissolved in deuterated chloroform), and the corresponding signal peaks of aliphatic polyamines and aromatic rings will be obtained, and the actual molecular weight can also be calculated. The theoretical molecular weight of each product can be calculated from the molar ratio of the raw materials. As shown in Table 1, the theoretical molecular weight is close to the actual molecular weight, indicating that the reaction is very complete.

[0098] In Table 1, the raw material examples (7), (17), (19) and (20) use an excess of aromatic dialdehydes, and the terminal groups of the final products are hydroxyl groups; the remaining examples use an excess of aliphatic polyamines, and the terminal groups of the final products are amine groups. Because amine groups can absorb CO2, for the present invention, the amine group end-capping method is preferred.

[0099] This group of raw material preparation examples fully demonstrates that polyamine polymers containing aromatic rings can be obtained through the reaction of aliphatic polyamines and aromatic dialdehydes. During the reduction process of sodium borohydride, the Schiff base (-C=N-) is selectively reduced, and the structure of the aromatic ring is retained. In fact, as long as it is an aromatic dialdehyde, regardless of the structure and size of the aromatic ring, it can react with aliphatic polyamines (containing at least two primary amino groups) to generate the corresponding polyamine polymers containing aromatic rings.

[0100] Examples 1 to 20

[0101] In this group of examples, the aromatic ring-containing polyamine polymers prepared in the raw material preparation examples (1) to (20) are used to absorb CO2 to form adducts, as shown in Table 2. The sample code prefix x in Table 2 represents the molecular weight of the aromatic ring-containing polyamine polymer, such as 1.8k, 3.6k, etc.; the suffix "-CO2" represents CO2 adducts; the letters in the middle are composed of the codes of aliphatic polyamines and aromatic dialdehydes. Source of polyamine polymer: Original (1) refers to the raw material preparation example (1) (see Table 1), and the others are similar.

[0102] Table 2

[0103]

[0104] The preparation method of the CO2 adduct of the polyamine polymer in Table 2 is as follows: 1 part by mass of the polyamine polymer (the source is listed in Table 2) is dissolved in ethanol to obtain a 10% mass concentration of the polyamine polymer solution, which is put into a closed reactor, and 0.5 MPa of CO2 is introduced to react for 5 hours to obtain a white precipitate, the solvent is filtered out, and then the precipitate is vacuum dried at 40°C for 3 days, and then the precipitate is put into a closed reactor and 0.5 MPa of CO2 is introduced to maintain the pressure for 2 days to obtain the CO2 adduct of the polyamine polymer.

[0105] The theoretical CO2 content in Table 2 is calculated based on the amino content of the polyamine polymer, and each two amino groups absorb one molecule of CO2. The actual CO2 content is obtained by thermogravimetric testing. As can be seen from the table, the actual CO2 content is close to the theoretical CO2 content, which indicates that the polyamine polymer prepared by the present invention can fully absorb CO2 to form an adduct of CO2.

[0106] It should be noted that since Examples 12 and 18 use dialdehydes with alkyl side chains to prepare polyamine polymers, the resulting CO2 adducts themselves have octyl (C8) side chains, and the percentage noted in Table 2 is the grafting rate of the side chains. It should be noted that the grafting rate is defined as the molar percentage of the number of N atoms grafted with side chains to the total N atoms in the main chain of the polyamine polymer.

[0107] Embodiments 20 to 47

[0108] In this group of embodiments, some aromatic ring-containing polyamine polymers are selected for grafting to increase the dispersibility of their CO2 adducts in the polyurethane raw materials. The side chains may be at least one of the following:

[0109] (1) The side chain is polyethylene glycol, polypropylene oxide, polyoxetane, polytetrahydrofuran or polysiloxane, and the degree of polymerization is at least 1;

[0110] (2) The side chain contains a trimethylsilyl group;

[0111] (3) The side chain contains a hydrocarbon group having 1 to 22 carbon atoms;

[0112] (4) The side chain contains a fluorinated alkyl group having 1 to 22 carbon atoms.

[0113] The grafting degree of the grafted side chain can be changed as needed, and can vary between 0 and 45%. The grafting degree is 0, that is, no grafting. Table 2 is a CO2 adduct foaming agent with a grafting degree of 0; therefore, this group of embodiments does not involve the case where the embodiment is 0.

[0114] Specifically, the structure of the synthesized grafted modified polyamine polymer is shown in Table 3. The theoretical grafting degree is calculated by the molar ratio of the amino groups grafted with side chains to all the amino groups on the main chain, and the actual grafting degree is calculated by the area ratio of the proton signals related to the side chains and the main chain in the nuclear magnetic resonance spectrum. It should be noted that the sample codes in the table are composed of the codes of the side chains and the polyamine polymers. In order to save space in the table, the suffix "-CO2" is omitted from the codes of all CO2 adducts, such as 10%C8-1.8kPEIP, where 10%C8 means that the side chain is an alkyl chain containing 8 carbon atoms, 10% represents the designed grafting degree of the side chain (i.e., the theoretical grafting degree), and 1.8kPEIP represents a benzene ring-containing polyamine polymer with a molecular weight of 1800, which is derived from the raw material preparation example (1). The source of the side chain is C8-EPO, and its structure is shown in Figure 5 The codes of other samples have similar meanings. Some samples have two grafted side chains, and the theoretical grafting degree and side chain code of each side chain are listed separately. All side chain raw materials are listed in Figure 5 middle.

[0115] The process conditions and steps for preparing aromatic ring-grafted polyamine polymers in Examples 21 to 42, 46 and 47 in Table 3 are as follows: the corresponding aromatic ring-containing polyamine polymer is added to a reactor, and ethanol is added to the reactor to make the mass concentration of the polyamine polymer about 10%, the polyamine polymer is completely dissolved under stirring, and then the corresponding glycidyl ether compound (Table 3, side chain raw material) is added to make the theoretical grafting degree of the side chain conform to the values ​​listed in Table 3, the reaction is stirred at 50°C for 15 hours, and then the ethanol is removed by rotary evaporation; then 10 parts by volume of petroleum ether is added to the product after rotary evaporation to dissolve the product and unreacted glycidyl ether compounds, and then 1 / 3 of distilled water is added based on the volume of petroleum ether to precipitate the grafted modified polyamine polymer; the precipitated polyamine polymer is washed with petroleum ether at least three times, and then the petroleum ether is removed by rotary evaporation and dried to constant weight to obtain the product.

[0116] The process conditions and steps of Example 43 in Table 3 are as follows: 1 mol of the aromatic ring-containing polyamine polymer prepared in Example (16) (i.e., 68.5 mol parts) was dissolved in chloroform to a mass concentration of about 10%, and then 0.03 mol of C 17 H 33 -COOH( Figure 5 ) and N,N'-carbonyldiimidazole (CDI), the theoretical grafting rate is 3%. Then the reaction is stirred under reflux for 12 hours, extracted with saturated brine three times, the chloroform layer is taken, the solvent is removed by rotary evaporation at 50°C, and finally dried in an oven at 75°C to obtain a purified hydrophobic linker grafted polyamine polymer product 3% C 17 H 33 -3.1kPBEIP.

[0117] The process conditions and steps of Example 44 in Table 3 are as follows: 1 mol of the aromatic ring-containing polyamine polymer (i.e., 58.0 parts by mass) prepared in Example (17) of the raw material preparation based on the N element contained was dissolved in chloroform to a mass concentration of about 10%, and then 0.2 mol of C2F3-I( Figure 5 ), reflux for 3 hours, cool to room temperature, extract the reaction mixture three times with a 5% sodium hydroxide aqueous solution with an equal volume to chloroform, remove the water layer, wash with water until the pH value of the water layer is neutral, dry the organic layer with anhydrous sodium sulfate, and remove the solvent by vacuum rotary evaporation at 40°C to obtain a hydrophobic chain-modified polyamine polymer 20% C2F3-3.6kPEIFP.

[0118] Table 3

[0119]

[0120] The process conditions and steps for preparing an aromatic ring grafted polyamine polymer in Example 45 in Table 3 are as follows: Take 1 mole of an aromatic ring-containing polyamine polymer (i.e., 54.2 parts by mass) prepared in Raw Material Preparation Example (2) based on the N element contained, and dissolve it in chloroform to make its mass concentration about 10%, then add 0.45 mole of C4-Br (Table 3), reflux for 6 hours, cool to room temperature, extract the reaction mixture three times with an equal volume of 5% sodium hydroxide aqueous solution as chloroform, remove the water layer, wash with water until the pH value of the water layer is neutral, dry the organic layer with anhydrous sodium sulfate, and remove the solvent by vacuum rotary evaporation at 40°C to obtain the corresponding hydrophobic chain modified polyamine polymer 45% C4-3.6kPEIP.

[0121] It can be seen from Table 3 that the actual grafting degree of each product is very close to the theoretical grafting degree, indicating that the grafting reaction is very complete. The theoretical grafting degree is calculated by the ratio of the molar number of the side chain to the molar number of the main chain nitrogen atoms, and the actual grafting degree is calculated by the area ratio of the proton signals related to the side chain and the main chain in the nuclear magnetic resonance spectrum. It can be seen from Table 3 that the grafting degree of the hydrophobic chain of each product is between 1 and 45%.

[0122] The preparation process and steps of the CO2 adducts of the grafted polyamine polymers in Table 3 are as follows: Each grafted polyamine polymer containing an aromatic ring is evenly spread on the surface of a glass container, and a CO2 gas flow is blown for 5 minutes, during which the viscous liquid gradually turns into a white solid. All the prepared CO2 adducts are placed in a pressure-maintaining container and reacted with CO2 for 24 hours under 0.6 MPa to obtain each product.

[0123] Figure 6 The infrared spectra of the CO2 adduct blowing agents prepared in Examples 2, 21 to 26 are 1629, 1557, 1466 and 1406 cm –1 The series of strong I peaks at 1115cm are attributed to the alkylammonium N–H bending vibration, carbamate C=O stretching vibration, and the asymmetric and symmetric skeleton stretching vibrations of the carbamate anion. –1 The peak is caused by the C–O–C stretching vibration on the side chain (indicated by *, Figure 6 ). N–H stretching vibration at 3425 cm -1 The aliphatic C–H stretching vibrations appear at 2929 and 2819 cm -1 Infrared spectroscopy confirmed that the synthesis of CO2 adduct was successful.

[0124] The theoretical CO2 content in Table 3 is calculated based on the amine content of the grafted polyamine polymer, and every two amine groups absorb one molecule of CO2. The actual CO2 content is obtained by thermogravimetric testing. All CO2 adducts have obvious thermogravimetric loss between 40 and 150°C, which can be attributed to the release of CO2. As can be seen from the table, the actual CO2 content is close to the theoretical CO2 content, which shows that the grafted polyamine polymer prepared by the present invention can fully absorb CO2 to form CO2 adducts.

[0125] Application Examples [1] to

[21] and Comparative Application Examples 1 to 5

[0126] This group of application examples selects CO2 adducts of some polyamine polymers containing aromatic rings for polyurethane foaming to verify its foaming effect. The formulas of each application example are shown in Table 4 (this formula is only used to illustrate the foaming effect of different foaming agents, and the foaming agent formula can be adjusted according to different purposes of use).

[0127] Table 4

[0128]

[0129] In Table 4, Polycin M-365 is a castor oil-derived polyol from Guangzhou Haoyi New Materials Technology Co., Ltd.; polyether 4110 is from Zibo Noli Chemical Co., Ltd., and propylene glycol is from Chengdu Changlian Chemical Reagent Co., Ltd.; dimethyl methyl phosphate is from Yangzhou Chenhua New Materials Co., Ltd.; stannous octoate and triethylenediamine are from Chengdu High-end Polymer Technology Co., Ltd.; the foaming agent BL-2580 is from Shanghai Maihao New Materials Technology Co., Ltd.; PM-200 is polymethylene polyphenyl isocyanate from Wanhua Chemical Group Co., Ltd., with an NCO content of 30.5-32.0%; the blowing agent is a homemade CO2 adduct of an aromatic ring-containing polyamine polymer, which is from Examples 1-47, as shown in Table 5.

[0130] In Table 5, the serial number “Comparative Example 1” refers to comparative example 1, and the same applies to the others; the serial number “[1]” refers to application example [1], and the same applies to the others; “Example 21” refers to Example 21, and the same applies to the others.

[0131] In Table 5, Comparative Examples 1, 3 and 4 do not add any foaming agent, and use the trace amount of water in the raw materials for foaming. Comparative Examples 2 and 5 use the CO2 adduct of branched polyethyleneimine (molecular weight 2500, from Shanghai Gongbi Ke New Materials Co., Ltd.) as the foaming agent. The preparation methods of 10% C8-PEI-CO2 (Comparative Example 2) and 10% C8-3.6kPEIP-CO2 (Example 22) are the same; the preparation methods of 10% PPG-PEI-CO2 (Comparative Example 5) and 10% PPG-3.6kPEIP-CO2 (Example 30) are the same.

[0132] Before preparing the foam, the dispersibility of different blowing agents in the macromolecular polyol was observed. Take 0.1g of each blowing agent (Table 5, comparative application examples 2 and 5, application examples [1] to

[13] and

[16] to

[19] ) and add it to 4.9g Polycin M-365 or polyether 4110. Stir magnetically at 300 rpm for 1 minute to obtain a turbid suspension. Use a digital camera to record the appearance of the solution. Store it at room temperature for 3 days and 7 days and record the changes in appearance again. At the same time, use an optical microscope to observe the morphology of the blowing agent particles in the white material. The results are as follows: Figure 7 and Figure 8 shown. Figure 7 Compatibility of alkyl chain-grafted blowing agents in bio-based polyol Polycin M-365. Blank samples without blowing agents are always transparent. At 0 days, all samples with CO2 adduct blowing agents are turbid and contain irregular particles of different sizes, while the transparency of samples with blowing agents increases after aging for 3 days. 10% C8-PEI-CO2 and 5% C8-3.6kPEIP-CO2 samples are translucent (indicated by *), 10% C8-1.8kPEIP-CO2 and 3.6kPEIP-CO2 samples have some sediment at the bottom (indicated by #), and the rest of the samples are as transparent as the blank samples (arrows indicate that the dents in the corners behind the samples can be clearly seen). From the overall analysis, it can be seen that the main chain molecular weight of the polyamine polymer (PEIP) containing benzene rings in the left group of samples is different, and the dispersibility increases with the increase of molecular weight (as the molecular weight increases, the benzene ring content also increases); the grafting rates of the right group of samples are different, and a higher grafting rate (such as 10% and 15%) is beneficial to improving the dispersibility of the foaming agent.

[0133] Table 5

[0134]

[0135] Figure 8The compatibility of the foaming agent grafted with dipropylene glycol methyl ether (mPPG2) in polyether 4110. The control sample does not contain any foaming agent (blank), and it has been clear and transparent during the placement period, and no particles can be seen under the microscope. At 0 days, the samples with the addition of foaming agent are all turbid in appearance, and no obvious difference can be seen. Under the microscopic state, it can be seen that the particle size of the particles in the ungrafted 3.6kPEIP-CO2 sample is larger, and the sample with a grafting rate of 5% can also observe particles with relatively large particle size. It was observed that under the same grafting rate, the particle size in the 10% PPG-3.6kPEI-CO2 sample is smaller than that in the 10% PPG-PEI-CO2, indicating that the foaming agent prepared with PEIP containing benzene rings has better compatibility than the foaming agent prepared with PEI without aromatic rings. When the grafting rate increases to 15%, it can be seen that the foaming agent is elliptical or round in polyether 4110, and the interface is smooth, indicating good compatibility. After 3 days, it can be seen that both the non-grafted and 5% grafted PEIP foaming agent samples have obvious precipitation ( Figure 8 , arrow), indicating that there are large particles in the sample, and sedimentation occurred during the static process, while the other three samples with added foaming agent are still turbid and opaque. In addition, it can be seen that with the passage of time, the particle size of each sample becomes smaller, and the sample with the best grafting rate of 15% basically has no obvious particles, while the sample with a grafting rate of 10%, which is slightly inferior, can see some small particles. From this, it can be concluded that the higher the grafting rate, the better the compatibility. At the same time, by comparing the foaming agents based on PEI and PEIP, it can be seen that PEIP has a better effect and contains smaller and more uniform particles. This is because the introduction of benzene rings in the PEI main chain can increase the lipophilicity of the foaming agent, thereby increasing the dispersibility of the foaming agent in the polyol.

[0136] Although different foaming agents have different dispersibility in macromolecular polyols, these foaming agents can all prepare polyurethane foams, and the formula is shown in Table 5. The blank sample is the foam produced without adding a foaming agent, which is mainly caused by the trace amount of water in the polyurethane raw material acting as a foaming agent. The specific foaming steps are: prepare the white material containing the foaming agent in a disposable plastic cup according to Formula I, Formula II and Formula III (Table 4), stir at 1200 rpm for 1 minute, then add PM-200 (black material), stir at 1200 rpm for 30 seconds, mix evenly, at this time the mixture becomes thick and white, put it in a drying oven at 80°C, the foam rises freely, and the height does not change after about 30 seconds, and then continue to mature for 30 minutes. The matured foam continues to be placed at room temperature for 3 days, and then the density and mechanical properties are tested.

[0137] Table 5 shows the density and mechanical properties of polyurethane foams prepared with different foaming agents (the data are the average values ​​of 5 tests). As can be seen from Table 5, the foam density of blank I is relatively large, while the density of foams with added foaming agents is correspondingly reduced (Comparative Example 2, Application Examples [1] to [9]); the foams prepared with other formulas II and III also have the same pattern. This shows that the added foaming agents can play a role in foaming. The change in the mechanical properties of the foam is normal. Generally speaking, the greater the density, the higher the mechanical strength.

[0138] Application Examples

[22] and

[23]

[0139] It should be pointed out that the application examples [1] to

[21] for preparing polyurethane foam fully illustrate that the prepared CO2 adducts of aromatic ring-containing polyamine polymers can be used to prepare polyurethane foam. For polyurethane foaming systems where the white material needs to be stored for a long time, such as spray insulation materials, the aromatic ring-containing foaming agent prepared by the present invention has better dispersibility in the white material and shows good redispersibility. We dispersed three foaming agents, 10% C8-PEI-CO2 (traditional grafted modified PEI), 3.6kPEIP-CO2 (polyamine polymer containing benzene ring, not grafted, from Example 2) and 10% C8-3.6kPEIP-CO2 (grafted polyamine polymer containing benzene ring, from Example 22) in castor oil-based polyol (Polycin M-365) (mass concentration 5%). The first two showed precipitation after 30 days, while the third foaming agent showed precipitation after 3 months. We continued to store for 180 days, and all three foaming agents precipitated to the bottom. The precipitate of the 10% C8-PEI-CO2 sample was severely agglomerated, and the foaming agent could not be redispersed by stirring; the latter two foaming agents (containing benzene rings) were easily dispersed into the body by stirring to re-form a uniform foaming mixture. This shows that the introduction of aromatic rings greatly increases the redispersibility of the foaming agent (even without grafting side chains). This good redispersibility can ensure the long-term storage stability of the white material system. Similarly, we compared the long-term dispersibility of 10% PPG-PEI-CO2 (Comparative Example 5) and 10% PPG-3.6kPEIP-CO2 (Example 30) in polyether 4110 (mass concentration 5%). The former showed stratification in about 20 days; the latter showed stratification in 30 days. After 180 days of long-term storage, the former could not be dispersed; the latter could disperse the foaming agent at the bottom evenly into the system by stirring. This shows that for the polyether system, the introduction of aromatic rings will also enhance the dispersibility of the foaming agent, and even if stratification occurs, it can be redispersed in the system.

[0140] To this end, we enlarged the white material formula of application examples [2] (foaming agent 10% C8-3.6kPEIP-CO2 in Polycin M-365) and

[18] (foaming agent 10% PPG-3.6kPEIP-CO2 in polyether 4110) by 100 times, stored it for 90 days, took out the white material at different times, foamed it according to the process of application examples [2] and

[18] , and tested the density and mechanical properties of the obtained foam. The results are shown in Table 6.

[0141] From the data in Table 6, it can be seen that both white materials can produce foam normally after long-term storage. The density and compression strength gradually decrease with the extension of storage time. This is because the white material absorbs a certain amount of water during storage, and the water plays a foaming role. If stored under strict isolation of water vapor, its foaming performance can remain stable. When polyethyleneimine without aromatic rings is used to prepare the corresponding foaming agent, the foaming agent precipitates within one month and cannot be dispersed again, and does not have long-term storage stability.

[0142] Table 6

[0143]

[0144] In addition, from Figure 7 and 8 From the observation of dispersibility, it can be seen that the compatibility of the foaming agent prepared by the present invention in castor oil-based polyols (some have been completely dissolved into a transparent state) is better than that in polyether polyols (no transparent state appears), indicating that the foaming agent of the polyamine polymer containing aromatic rings is more suitable for plant oil-based polyols, which lays a good foundation for the next generation of carbon-neutral polyurethane foams.

[0145] The above description is only an embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent substitution, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of the claims of the present invention.

Claims

1. A graft modified polyamine polymer CO 2 The use of the adduct foaming agent is used to prepare a polyurethane foaming white material containing polyether 4110, and the white material has a storage period of 90 days and can be used for the preparation of polyurethane foam; the CO of the grafted polyamine polymer 2 Adduct blowing agent is composed of grafted polyamine polymer and CO 2 The grafted polyamine polymer and CO 2 An adduct is formed, and the main chain structure of the grafted polyamine polymer is: in, R 1 It is the structure obtained by removing the terminal primary amine group of pentaethylenehexamine; R 2 The structure obtained by removing the aldehyde group from terephthalaldehyde, namely R 2 is a benzene ring; n is an integer not less than 1, and the average molecular weight of the polyamine polymer is 3.6 kDa; the terminal group of the polyamine polymer is an amine group; The side chain of the grafted polyamine polymer is polypropylene oxide, and the degree of polymerization is 2; The grafting rate of the grafted polyamine polymer is 10 mol % based on the N atoms in the main chain of the polyamine polymer.

2. A graft modified polyamine polymer CO 2 The use of the adduct foaming agent is used to prepare a polyurethane foaming white material containing bio-based polyol Polycin M-365, which has a storage period of 90 days and can be used for the preparation of polyurethane foam; the CO of the grafted polyamine polymer 2 Adduct blowing agent is composed of grafted polyamine polymer and CO 2 The grafted polyamine polymer and CO 2 An adduct is formed, and the main chain structure of the grafted polyamine polymer is: in, R 1 It is the structure obtained by removing the terminal primary amine group of pentaethylenehexamine; R 2 The structure obtained by removing the aldehyde group from terephthalaldehyde, namely R 2 is a benzene ring; n is an integer not less than 1, and the average molecular weight of the polyamine polymer is 3.6 kDa; the terminal group of the polyamine polymer is an amine group; The side chain of the grafted polyamine polymer contains an alkyl group with 8 carbon atoms; The grafting rate of the grafted polyamine polymer is 10 mol % based on the N atoms in the main chain of the polyamine polymer.

Citation Information

Patent Citations

  • CO2 absorbent of hydrophobic modified polyethyleneimine and application

    CN108355472A

  • Aromatic nucleus-containing polyamine polymer for releasing carbon dioxide foaming agent

    CN116769120A