A high calorific value biomass fuel

Through crushing, decomposition removal, fermentation and catalytic treatment, combined with extrusion molding technology of materials such as urea and formaldehyde resin, the calorific value and bonding strength of biomass fuel are improved, and the problems of low calorific value and large molding energy consumption are solved. , realizes efficient biomass fuel preparation.

CN116804158BActive Publication Date: 2024-11-29JIANGXI ZIFENG JEWELRY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310844344.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-11
Publication Date
2024-11-29
Estimated Expiration
2043-07-11

AI Technical Summary

Technical Problem

The calorific value of biomass fuel is low and consumes a lot of energy during molding, and has poor bonding strength and density, which affects storage and combustion efficiency.

Method used

Using the steps of crushing, decomposition, fermentation, drying, catalytic and extrusion molding, high-calorie biomass is formed by chemicals such as hydrolase, yeast, zinc triflate, urea-formaldehyde resin and anti-slag agent. fuel.

Benefits of technology

It significantly improves the calorific value and bonding strength of biomass fuel, reduces the energy consumption of the molding process, and enhances combustion efficiency and storage stability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a high calorific value biomass fuel, wherein the calorific value of the biomass is increased by fermenting the biomass and performing subsequent reaction treatment, the bonding performance of the urea-formaldehyde resin and the water resistance of the biomass fuel are enhanced by modifying the binder urea-formaldehyde resin, and the shrinkage rate of the urea-formaldehyde resin is also reduced, and finally the slagging rate of the biomass fuel is further reduced by modifying the activated clay and coating it with calcium percarbonate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomass fuels, and in particular relates to a high calorific value biomass fuel. Background Art

[0002] Biomass fuel refers to the burning of biomass materials as fuel, generally mainly agricultural and forestry wastes such as straw, sawdust, bagasse and rice husks. The application of biomass fuel is actually mainly biomass molded fuel, which uses agricultural and forestry waste as raw materials and is prepared into blocks or granules through processes such as crushing, mixing, extrusion and drying to form a new type of clean fuel that can be directly burned.

[0003] Although biomass fuel is a new type of clean fuel, its calorific value is still far behind that of traditional fossil energy sources such as coal and oil. At the same time, since biomass fuel contains a certain amount of water, it is not easy to burn fully, which also affects its calorific value to a certain extent.

[0004] There are mainly two types of biomass fuel molding: hot pressing molding and room temperature molding. Hot pressing molding of biomass fuel requires high temperature and high pressure, and consumes a lot of energy. The molding pressure of room temperature molding of biomass fuel is greater than that of hot pressing molding, but its bonding strength and density after molding are not as good as those of hot pressing molding. Therefore, the calorific value of room temperature molding biomass fuel is not as good as that of hot pressing molding biomass fuel, and it is also not easier to store than hot pressing molding biomass fuel.

[0005] Therefore, a method for preparing high calorific value biomass fuel is needed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing high calorific value biomass fuel.

[0007] In order to solve the above technical problems, the technical solution adopted by the present invention comprises the following steps:

[0008] A high calorific value biomass fuel, the specific preparation steps are:

[0009] (1) The straw is crushed using a pulverizer, and particles with a particle size of less than 3 mm are retained after screening. The particles are then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water are mixed at a solid-liquid ratio of 1:5-7 (g / mL), and 0.3-0.5% of the mass of particles a hydrolase is added at the same time. The reaction is carried out for 2-4 hours to obtain reactant a;

[0010] (2) Adding reactant a into a fermentation tank, adding yeast of 0.2-0.4% by weight of particle a and 1-2 parts of fermentation accelerator, and performing anaerobic fermentation at 30-32° C. for 2-3 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0011] (3) adding the dried solid a, liquid a and 1-2 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 80-90° C. and 0.2-0.3 MPa for 2.5-3.5 hours to obtain product a after the reaction is completed;

[0012] (4) First, 0.6-1 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride are mixed evenly, and then product a and 1-1.2 parts of an anti-slagging agent are added and mixed evenly, and then extruded at 50-55°C and 16-20MPa to obtain biomass molded fuel.

[0013] Furthermore, the method for preparing the fermentation promoter in step (2) is:

[0014] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.5-6.7.

[0015] Furthermore, the urea-formaldehyde resin in step (4) further includes the following treatment method:

[0016] (1) Add 0.3-0.5% of the mass of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a dilute solution with a concentration of 0.9-1.1% to obtain a modified solution;

[0017] (2) polyoxyethylene hydrogenated castor oil and anhydrous ethanol are mixed in a volume ratio of 1:2.5-3.5 to obtain a coating solution, and then 6-10 μm wollastonite is immersed in the coating solution for 3-5 minutes, followed by drying to remove the anhydrous ethanol, and this cycle is repeated three times to obtain a modifier;

[0018] (3) The urea-formaldehyde resin, the modifying liquid and the modifying agent are uniformly mixed in a mass ratio of 1:0.2~0.3:0.1~0.2 to obtain the modified urea-formaldehyde resin.

[0019] Furthermore, the anti-slagging agent in step (4) is prepared by mixing activated clay and calcium percarbonate in a mass ratio of 5:3.

[0020] Furthermore, the activated clay also includes the following treatment method:

[0021] Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred to obtain a suspension, and then 0.7% to 0.8% of tetrabutylammonium hexafluorophosphate by mass of the activated clay was added, and the pH value was adjusted to 10.4 to 10.8 after stirring, and then the temperature was raised to 80 to 90°C for reaction for 3 to 4 hours. After the reaction was completed, the filter was filtered, and the filter cake was washed three times with anhydrous ethanol, followed by drying and crushing to obtain the modified activated clay.

[0022] Furthermore, the calcium percarbonate also includes the following processing method:

[0023] The coating liquid a is obtained by uniformly mixing hydrogenated rosin glycerol ester and acetone in a mass ratio of 1:1-2, and then the calcium percarbonate is immersed in the coating liquid a for 2-4 minutes, followed by drying at 24-26°C. This cycle is repeated three times to obtain the coated calcium percarbonate.

[0024] The beneficial effects of the present invention are:

[0025] (1) After N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid is configured into a buffer solution, it can stabilize the pH value of the fermentation system, thereby ensuring the stability and activity of the microorganisms. Compared with conventional buffer solutions such as acetic acid buffer solutions, N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid has a stronger polarity to promote the fermentation reaction. N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid has a certain complexing property and can remove some heavy metals in biomass. At the same time, N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid is non-toxic to microorganisms and will not affect the fermentation process.

[0026] (2) Compared with conventional acid catalysts such as sulfuric acid, zinc trifluoromethanesulfonate has stronger catalytic performance, which can make the reaction conditions milder and the reaction time shorter. At the same time, zinc trifluoromethanesulfonate is not highly acidic after being dissolved in water, and has a weaker corrosive effect on the reaction equipment. At the same time, zinc trifluoromethanesulfonate will not undergo redox reactions and will not have side reactions with the reactants, thereby affecting the performance of the product.

[0027] (3) The effect of directly adding KH-560 and wollastonite to urea-formaldehyde resin is not obvious, and the water resistance and shrinkage rate of urea-formaldehyde resin are not significantly improved. After mixing perfluoropolyether-based surfactant and KH-560, on the one hand, the dispersibility of KH-560 in urea-formaldehyde resin can be enhanced, so that KH-560 can fully react with urea-formaldehyde resin to enhance the water resistance of urea-formaldehyde resin. On the other hand, the viscosity of urea-formaldehyde resin can be adjusted to make it better bonded with biomass fuel. At the same time, perfluoropolyether-based surfactant can form a dense fluorinated surface layer on the surface of biomass fuel after biomass fuel is formed, further enhancing the water resistance of biomass fuel.

[0028] (4) After wollastonite is coated with polyoxyethylene hydrogenated castor oil, on the one hand, the compatibility of wollastonite in urea-formaldehyde resin can be enhanced, and wollastonite can be evenly dispersed in urea-formaldehyde resin during stirring. On the other hand, the coating also has a sustained release effect. After wollastonite is evenly dispersed in urea-formaldehyde resin, polyoxyethylene hydrogenated castor oil will slowly dissolve in the water contained in urea-formaldehyde resin during stirring. After polyoxyethylene hydrogenated castor oil is completely dissolved, wollastonite can continue to cross-link with KH-560, further enhancing the bonding strength and other properties of urea-formaldehyde resin. At the same time, polyoxyethylene hydrogenated castor oil dissolved in water can also stabilize the resin before urea-formaldehyde resin is cured.

[0029] (5) Tetrabutylammonium hexafluorophosphate can stabilize the interlayer structure through intercalation reaction to improve its adsorption performance. At the same time, tetrabutylammonium hexafluorophosphate can also be applied to the surface of activated clay by physical adsorption. Tetrabutylammonium hexafluorophosphate has the effect of ion pair reagent and can also bind to some alkali metals. At the same time, because hexafluorophosphate has a strong electronegativity, it can also enhance the adsorption performance of activated clay.

[0030] (6) Calcium percarbonate is easy to decompose in the presence of water and high temperature. After being coated with hydrogenated rosin glycerol ester, it can isolate moisture on the one hand and have a heat insulation effect on the other hand. Even if calcium percarbonate decomposes due to temperature during the biomass molding process, the oxygen produced by the decomposition can be retained inside. At the same time, hydrogenated rosin glycerol ester will also be slightly softened during the molding process. In this process, it also has the effect of enhancing the bonding strength of biomass molding fuel. In the process of biomass combustion, hydrogenated rosin glycerol ester can also be used as a combustible to promote combustion. DETAILED DESCRIPTION

[0031] The present invention will be further described in detail below in conjunction with the embodiments. Example 1

[0032] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.6 to obtain a fermentation promoter.

[0033] The anti-slagging agent is obtained by mixing activated clay and calcium percarbonate in a mass ratio of 5:3.

[0034] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0035] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0036] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0037] (4) First, 0.8 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel. Example 2

[0038] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.5 to obtain a fermentation promoter.

[0039] The anti-slagging agent is obtained by mixing activated clay and calcium percarbonate in a mass ratio of 5:3.

[0040] (1) The straw was crushed using a pulverizer, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:7 (g / mL), and 0.3% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 4 hours to obtain reactant a.

[0041] (2) Adding reactant a into a fermentation tank, adding yeast of 0.2% by weight of particle a and 2 parts of fermentation accelerator, and carrying out anaerobic fermentation at 32°C for 2 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0042] (3) adding the dried solid a, liquid a and 1 part of zinc trifluoromethanesulfonate into a reactor, and then reacting at 90° C. and 0.2 MPa for 2.5 h, and obtaining product a after the reaction is completed;

[0043] (4) First, 0.6 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.2 parts of anti-slagging agent were added and mixed evenly, and then extruded at 55°C and 16MPa to obtain biomass molded fuel. Example 3

[0044] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.7 to obtain a fermentation promoter.

[0045] The anti-slagging agent is obtained by mixing activated clay and calcium percarbonate in a mass ratio of 5:3.

[0046] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:5 (g / mL), and 0.5% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 2 hours to obtain reactant a.

[0047] (2) Adding reactant a into a fermentation tank, adding yeast of 0.4% by weight of particle a and 1 part of fermentation accelerator, and carrying out anaerobic fermentation at 30°C for 3 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0048] (3) adding the dried solid a, liquid a and 1-2 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 80° C. and 0.3 MPa for 3.5 hours to obtain product a after the reaction is completed;

[0049] (4) First, 1 part of urea-formaldehyde resin and 0.6% by weight of ammonium chloride are mixed evenly, and then product a and 1 part of anti-slagging agent are added and mixed evenly, and then extruded at 50°C and 20MPa to obtain biomass molded fuel. Example 4

[0050] Dissolve 3 parts of acetic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.6 to obtain a fermentation promoter.

[0051] The rest is the same as in Example 1. Example 5

[0052] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0053] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0054] (3) The dried solid a, liquid a and 1.5 parts of sulfuric acid are added into a reactor, and then reacted at 85°C and 0.25 MPa for 3 hours. After the reaction is completed, product a is obtained;

[0055] (4) First, 0.8 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel.

[0056] The rest is the same as in Example 1. Example 6

[0057] (1) The straw is crushed by a crusher, and particles with a particle size of less than 3 mm are retained after screening, and then the particles are placed in a de-impurity device to remove impurities to obtain particles a;

[0058] (2) 20 parts of granules a were added into a fermentation tank, and yeast at a weight percentage of 0.3% of the weight of granules a and 1.5 parts of a fermentation accelerator were added at the same time, and anaerobic fermentation was carried out at 31° C. for 2.5 days. After the fermentation was completed, solid a and filtrate a were obtained by filtration, and the solid a was dried. Dicyclohexylcarbodiimide was added to the filtrate a, and then liquid a was obtained by filtration;

[0059] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0060] (4) First, 0.8 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel.

[0061] The rest is the same as in Example 1. Example 7

[0062] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0063] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 44°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0064] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0065] (4) First, 0.8 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel.

[0066] The rest is the same as in Example 1. Example 8

[0067] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0068] (2) Adding reactant a into a fermentation tank, adding yeast at 0.3% of the mass of particle a and 1.5 parts of a fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, and drying the solid a;

[0069] (3) adding the dried solid a, filtrate a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0070] (4) First, 0.8 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel.

[0071] The rest is the same as in Example 1. Example 9

[0072] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0073] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0074] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 110° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0075] (4) First, 0.8 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel.

[0076] The rest is the same as in Example 1.

[0077] The biomass fuels prepared in Examples 1 to 9 were tested for calorific value according to GB / T 30727-2014 “Method for determination of calorific value of solid biomass fuels”. Specific data are shown in Table 1.

[0078] Table 1 Calorific value of biomass fuel in each example

[0079] Implementation items Calorific value (MJ / kg) Example 1 23.91 Example 2 23.74 Example 3 23.82 Example 4 18.88 Example 5 18.97 Example 6 19.76 Example 7 20.84 Example 8 21.68 Example 9 20.19

[0080] As can be seen from Table 1, the calorific values ​​of Examples 1 to 3 are the highest; among them, Examples 4 and 5 replaced the fermentation promoter and the catalyst respectively, and their calorific values ​​are at the lowest level; the calorific value of Example 6 is also significantly lower than that of Example 1, which may be due to the fact that no hydrolysis was performed, and the complex polysaccharides in the straw were not converted into simple polysaccharides. On the one hand, the carbon source required for microbial growth was reduced, and on the other hand, it took longer for the microorganisms to decompose the complex polysaccharides, which ultimately resulted in a poor fermentation effect; the reason why the calorific value of Example 7 is not high may be that the temperature during fermentation is too high, affecting the activity of the yeast; the calorific value of Example 8 is also lower than that of Example 1, which may be due to the fact that the moisture in the filtrate after fermentation was not removed, affecting the subsequent grafting reaction, and then affecting the calorific value of the biomass fuel; the reason for the lower calorific value in Example 9 may be that the grafting reaction temperature is too high. On the one hand, ethanol will become a gas due to reaching the boiling point, and on the other hand, the excessively high temperature may also cause side reactions, affecting the progress of the grafting reaction, thereby affecting the calorific value of the biomass fuel. Example 10

[0081] Add 0.4% of the mass of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a 1% dilute solution to obtain a modified solution;

[0082] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:3 to obtain a coating solution, and then 8 μm wollastonite was immersed in the coating solution for 4 minutes, and then the anhydrous ethanol was removed by drying, and this cycle was repeated 3 times to obtain a modifier;

[0083] The modified urea-formaldehyde resin is obtained by uniformly mixing the urea-formaldehyde resin, the modifying liquid and the modifying agent in a mass ratio of 1:0.25:0.15.

[0084] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.6 to obtain a fermentation promoter.

[0085] The anti-slagging agent is obtained by mixing activated clay and calcium percarbonate in a mass ratio of 5:3.

[0086] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0087] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0088] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0089] (4) First, 0.8 parts of modified urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel. Embodiment 11

[0090] Add 0.3% of the mass of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a dilute solution with a concentration of 1.1% to obtain a modified solution;

[0091] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:2.5 to obtain a coating solution, and then 10 μm wollastonite was immersed in the coating solution for 3 minutes, and then the anhydrous ethanol was removed by drying, and this cycle was repeated 3 times to obtain a modifier;

[0092] The modified urea-formaldehyde resin is obtained by uniformly mixing the urea-formaldehyde resin, the modifying liquid and the modifying agent in a mass ratio of 1:0.3:0.1.

[0093] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.6 to obtain a fermentation promoter.

[0094] The anti-slagging agent is obtained by mixing activated clay and calcium percarbonate in a mass ratio of 5:3.

[0095] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0096] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0097] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0098] (4) First, 0.8 parts of modified urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel. Example 12

[0099] Add 0.5% of the mass of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a dilute solution with a concentration of 0.9% to obtain a modified solution;

[0100] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:3.5 to obtain a coating solution, and then 6 μm wollastonite was immersed in the coating solution for 5 minutes, and then the anhydrous ethanol was removed by drying, and this cycle was repeated 3 times to obtain a modifier;

[0101] The modified urea-formaldehyde resin is obtained by uniformly mixing the urea-formaldehyde resin, the modifying liquid and the modifying agent in a mass ratio of 1:0.2:0.2.

[0102] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.6 to obtain a fermentation promoter.

[0103] The anti-slagging agent is obtained by mixing activated clay and calcium percarbonate in a mass ratio of 5:3.

[0104] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0105] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0106] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0107] (4) First, 0.8 parts of modified urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel. Embodiment 13

[0108] Add 0.4% by weight of sodium dodecyl sulfate to KH-560, and then add water to make a 1% dilute solution to obtain the modified solution.

[0109] The rest is the same as Example 10. Embodiment 14

[0110] Sodium carboxymethyl cellulose and deionized water were mixed in a volume ratio of 1:3 to obtain a coating solution, and then 8 μm wollastonite was immersed in the coating solution for 4 minutes, followed by drying to remove the deionized water, and this cycle was repeated 3 times to obtain a modifier.

[0111] The rest is the same as Example 10. Embodiment 15

[0112] Add 1% by weight of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a 1% dilute solution to obtain a modified solution.

[0113] The rest is the same as Example 10. Example 16

[0114] Add 0.4% by weight of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a 4% dilute solution to obtain a modified solution.

[0115] The rest is the same as Example 10. Embodiment 17

[0116] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:6 to obtain a coating solution, and then 8 μm wollastonite was immersed in the coating solution for 4 minutes, followed by drying to remove the anhydrous ethanol, and this cycle was repeated three times to obtain a modifier.

[0117] The rest is the same as Example 10. Embodiment 18

[0118] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:3 to obtain a coating solution, and then 15 μm wollastonite was immersed in the coating solution for 4 minutes, followed by drying to remove the anhydrous ethanol, and this cycle was repeated 3 times to obtain a modifier.

[0119] The rest is the same as Example 10. Embodiment 19

[0120] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:3 to obtain a coating solution, and then 8 μm wollastonite was immersed in the coating solution for 8 minutes, followed by drying to remove the anhydrous ethanol, and this cycle was repeated three times to obtain a modifier.

[0121] The rest is the same as Example 10.

[0122] Part of the biomass fuel prepared in Examples 10 to 19 was placed in an environment with a temperature of 25°C and a humidity of 75% for 10 days, and then the mass m1 before placement and the mass m2 after placement were measured. The mass change rate was calculated by a formula a=(m2-m1) / m1, and the water resistance of the biomass fuel was evaluated by the mass change rate. The shrinkage rate was calculated by the formula b=(V1-V2) / V1, wherein V1 represents the volume before curing and V2 represents the volume after curing. At the same time, part of the biomass fuel prepared in Examples 10 to 19 was placed in a soft packaging bag and freely dropped from a height of 2m to a steel plate of a specified thickness or a hardened ground for a total of 5 drops. The proportion of biomass fuel with a mass change of less than 5% before and after the drop was measured, which was recorded as the crush resistance c. The specific data are shown in Table 2.

[0123] Table 2 Mechanical properties data of biomass fuels in Examples 10 to 19

[0124] Implementation items Quality change rate a (%) Shrinkage rate b (%) Crushing resistance c (%) Example 1 8.62 0.94 78.7 Example 10 0.21 0.11 98.6 Embodiment 11 0.34 0.13 98.1 Example 12 0.32 0.14 97.3 Embodiment 13 5.14 0.16 93.3 Embodiment 14 0.46 0.79 85.3 Embodiment 15 0.36 0.17 92.7 Example 16 1.58 0.32 92.0 Embodiment 17 0.35 0.62 90.7 Embodiment 18 0.42 0.67 91.3 Embodiment 19 0.34 0.15 96.7

[0125] It can be seen from Table 2 that the mass change rate, shrinkage rate and compressive strength of the biomass fuel prepared in Examples 10 to 12 are all at the optimal level; the urea-formaldehyde resin was not modified in Example 1, so its three performance parameters were poor; the water resistance of Example 13 was poor, which may be because the replaced surfactant did not enhance the water resistance, and the dispersibility was weak, which in turn affected the biomass fuel's resistance to crushing; Example 14 replaced the coating material, and its resistance to crushing was significantly reduced compared with Example 10; the resistance to crushing of the biomass fuel prepared in Example 15 was slightly weakened compared with Example 10, which may be due to excessive addition of perfluoropolyether-based surfactant, which affected the curing of urea-formaldehyde resin, and then affected the biomass fuel's resistance to crushing; Example 16 was because the silane coupling agent Too high a concentration affects the water resistance and breakage resistance of the biomass fuel. The reason may be that the silane coupling agent concentration is too high, causing it to undergo self-polymerization reaction, thereby affecting the dispersibility and stability of the urea-formaldehyde resin; the reason for the high shrinkage rate and poor breakage resistance of Example 17 may be that the coating liquid concentration is too low, resulting in incomplete wollastonite coating, which in turn affects the dispersibility of wollastonite in urea-formaldehyde resin and causes wollastonite to react with the silane coupling agent in advance; the reason for the high shrinkage rate and poor breakage resistance of Example 18 may be that the wollastonite particle size is too large, affecting its dispersibility in urea-formaldehyde resin, and at the same time its specific surface area is also reduced, which ultimately affects the strength and shrinkage rate of the resin after curing; the performance data of Example 19 is not much different from that of Example 10, indicating that the coating immersion time of Example 10 is the optimal time. Embodiment 20

[0126] Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred evenly to obtain a suspension, and then 0.75% of tetrabutylammonium hexafluorophosphate by mass of the activated clay was added, and the pH value was adjusted to 10.6 after stirring evenly, and then the temperature was raised to 85°C for reaction for 3.5 hours. After the reaction was completed, the filter was filtered, and the filter cake was washed three times with anhydrous ethanol, and then dried and crushed to obtain modified activated clay.

[0127] The coating liquid a is obtained by uniformly mixing hydrogenated rosin glycerol ester and acetone in a mass ratio of 1:1.5, and then the calcium percarbonate is immersed in the coating liquid a for 3 minutes, followed by drying at 25°C. This cycle is repeated three times to obtain coated calcium percarbonate.

[0128] Add 0.4% of the mass of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a 1% dilute solution to obtain a modified solution;

[0129] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:3 to obtain a coating solution, and then 8 μm wollastonite was immersed in the coating solution for 4 minutes, and then the anhydrous ethanol was removed by drying, and this cycle was repeated 3 times to obtain a modifier;

[0130] The modified urea-formaldehyde resin is obtained by uniformly mixing the urea-formaldehyde resin, the modifying liquid and the modifying agent in a mass ratio of 1:0.25:0.15.

[0131] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.6 to obtain a fermentation promoter.

[0132] The modified activated clay and coated calcium percarbonate are mixed in a mass ratio of 5:3 to obtain an anti-slagging agent.

[0133] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0134] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0135] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0136] (4) First, 0.8 parts of modified urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel. Embodiment 21

[0137] Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred evenly to obtain a suspension, and then 0.7% of tetrabutylammonium hexafluorophosphate by mass of the activated clay was added, and the pH value was adjusted to 10.8 after stirring evenly, and then the temperature was raised to 80°C for reaction for 4 hours. After the reaction was completed, the filter was filtered, and the filter cake was washed three times with anhydrous ethanol, and then dried and crushed to obtain modified activated clay.

[0138] The coating liquid a is obtained by uniformly mixing hydrogenated rosin glycerol ester and acetone in a mass ratio of 1:1, and then the calcium percarbonate is immersed in the coating liquid a for 4 minutes, followed by drying at 24°C. This cycle is repeated three times to obtain coated calcium percarbonate.

[0139] Add 0.4% of the mass of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a 1% dilute solution to obtain a modified solution;

[0140] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:3 to obtain a coating solution, and then 8 μm wollastonite was immersed in the coating solution for 4 minutes, and then the anhydrous ethanol was removed by drying, and this cycle was repeated 3 times to obtain a modifier;

[0141] The modified urea-formaldehyde resin is obtained by uniformly mixing the urea-formaldehyde resin, the modifying liquid and the modifying agent in a mass ratio of 1:0.25:0.15.

[0142] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.6 to obtain a fermentation promoter.

[0143] The modified activated clay and coated calcium percarbonate are mixed in a mass ratio of 5:3 to obtain an anti-slagging agent.

[0144] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0145] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0146] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0147] (4) First, 0.8 parts of modified urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel. Embodiment 22

[0148] Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred evenly to obtain a suspension, and then 0.8% of tetrabutylammonium hexafluorophosphate by mass of the activated clay was added, and the pH value was adjusted to 10.4 after stirring evenly, and then the temperature was raised to 90°C to react for 3 hours. After the reaction was completed, the filter was filtered, and the filter cake was washed three times with anhydrous ethanol, and then dried and crushed to obtain modified activated clay.

[0149] The coating liquid a is obtained by uniformly mixing hydrogenated rosin glycerol ester and acetone in a mass ratio of 1:2, and then the calcium percarbonate is immersed in the coating liquid a for 2 minutes, followed by drying at 26°C. This cycle is repeated three times to obtain coated calcium percarbonate.

[0150] Add 0.4% of the mass of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a 1% dilute solution to obtain a modified solution;

[0151] Polyoxyethylene hydrogenated castor oil and anhydrous ethanol were mixed in a volume ratio of 1:3 to obtain a coating solution, and then 8 μm wollastonite was immersed in the coating solution for 4 minutes, and then the anhydrous ethanol was removed by drying, and this cycle was repeated 3 times to obtain a modifier;

[0152] The modified urea-formaldehyde resin is obtained by uniformly mixing the urea-formaldehyde resin, the modifying liquid and the modifying agent in a mass ratio of 1:0.25:0.15.

[0153] Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.6 to obtain a fermentation promoter.

[0154] The modified activated clay and coated calcium percarbonate are mixed in a mass ratio of 5:3 to obtain an anti-slagging agent.

[0155] (1) The straw was crushed using a crusher, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:6 (g / mL), and 0.4% of the mass of the particles a was added with a hydrolase. The reaction was carried out for 3 hours to obtain reactant a.

[0156] (2) Adding reactant a into a fermentation tank, adding yeast of 0.3% by weight of particle a and 1.5 parts of fermentation accelerator, and performing anaerobic fermentation at 31°C for 2.5 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a;

[0157] (3) adding the dried solid a, liquid a and 1.5 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 85° C. and 0.25 MPa for 3 h, and obtaining product a after the reaction is completed;

[0158] (4) First, 0.8 parts of modified urea-formaldehyde resin and 0.6% by weight of ammonium chloride were mixed evenly, and then product a and 1.1 parts of anti-slagging agent were added and mixed evenly, and then extruded at 52.5°C and 18 MPa to obtain biomass molded fuel. Embodiment 23

[0159] Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred evenly to obtain a suspension. Then, 0.75% of dodecyltrimethylammonium bromide by mass of the activated clay was added, and the pH value was adjusted to 10.6 after stirring evenly. The reaction was carried out for 3.5 hours. After the reaction was completed, the filter was filtered and the filter cake was washed three times with anhydrous ethanol, and then dried and crushed to obtain modified activated clay.

[0160] The rest is the same as Example 20. Embodiment 24

[0161] Paraffin wax and ether were mixed evenly at a mass ratio of 1:1.5 to obtain coating liquid a, and then calcium percarbonate was immersed in the coating liquid a for 3 minutes, followed by drying at 25°C. This cycle was repeated 3 times to obtain coated calcium percarbonate.

[0162] The rest is the same as Example 20. Embodiment 25

[0163] Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred to obtain a suspension, and then 0.75% of tetrabutylammonium hexafluorophosphate by mass of the activated clay was added, and the pH value was adjusted to 12 after stirring, and then the temperature was raised to 85°C for reaction for 3.5 hours. After the reaction was completed, the filter was filtered, and the filter cake was washed three times with anhydrous ethanol, and then dried and crushed to obtain modified activated clay.

[0164] The rest is the same as Example 20. Embodiment 26

[0165] Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred evenly to obtain a suspension, and then 0.75% of tetrabutylammonium hexafluorophosphate by mass of the activated clay was added, and the pH value was adjusted to 10.6 after stirring evenly, and then the temperature was raised to 100°C to react for 3.5 hours. After the reaction was completed, the mixture was filtered, and the filter cake was washed three times with anhydrous ethanol, followed by drying and crushing to obtain modified activated clay.

[0166] The rest is the same as Example 20. Embodiment 27

[0167] Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred to obtain a suspension, and then 0.75% of tetrabutylammonium hexafluorophosphate by mass of the activated clay was added, and the pH value was adjusted to 10.6 after stirring, and then the temperature was raised to 85°C for reaction for 5 hours. After the reaction was completed, the filter was filtered, and the filter cake was washed three times with anhydrous ethanol, and then dried and crushed to obtain modified activated clay.

[0168] The rest is the same as Example 20. Embodiment 28

[0169] The coating liquid a is obtained by uniformly mixing hydrogenated rosin glycerol ester and acetone in a mass ratio of 1:3, and then the calcium percarbonate is immersed in the coating liquid a for 3 minutes, followed by drying at 25°C. This cycle is repeated 3 times to obtain coated calcium percarbonate.

[0170] The rest is the same as Example 20. Embodiment 29

[0171] The coating liquid a is obtained by uniformly mixing hydrogenated rosin glycerol ester and acetone in a mass ratio of 1:1.5, and then the calcium percarbonate is immersed in the coating liquid a for 6 minutes, followed by drying at 25°C. This cycle is repeated three times to obtain coated calcium percarbonate.

[0172] The rest is the same as Example 20.

[0173] The slagging rates of the biomass fuels prepared in Example 1 and Examples 20 to 29 were measured according to NB / T 34025-2015 “Test Method for Slagging of Biomass Solid Fuels”. The specific data are shown in Table 3.

[0174] Table 3 Slagging rate of biomass fuel in various examples

[0175] Implementation items Slagging rate (%) Embodiment 20 1.59 Embodiment 21 1.71 Embodiment 22 1.66 Embodiment 23 6.83 Embodiment 24 6.15 Embodiment 25 2.94 Embodiment 26 3.93 Embodiment 27 3.67 Embodiment 28 2.48 Embodiment 29 1.70 Example 1 8.74

[0176] It can be seen from Table 3 that Examples 20 to 22 have the lowest slagging rates, indicating that their anti-slagging agents have the best effect; in Example 1, the activated clay was not modified and calcium percarbonate was not coated, so its slagging rate was the highest; in Example 23, tetrabutylammonium hexafluorophosphate was replaced by dodecyltrimethylammonium bromide, and its slagging rate was significantly increased compared with Example 20; in Example 24, the coating material hydrogenated rosin glycerol ester was replaced by paraffin, and its slagging rate was similar to that of Example 23; the reason for the increase in slagging rate in Example 25 may be that the pH value during the modification of the activated clay was increased, and the excessively high pH value inhibited the modification reaction, thereby affecting the modification effect; in Example 26, the activated clay was increased. Reaction temperature. Too high a reaction temperature may also inhibit the modification reaction and may also produce side reactions, so its slagging rate is also increased; Example 27 prolongs the reaction time of the activated white clay. Too long a reaction time may cause the chemical bonds generated by the reaction to break, thereby affecting the modification effect of the activated white clay; Example 28 increases the amount of solvent acetone. The reason for the increase in slagging rate may be that the low concentration of the coating liquid leads to incomplete coating of part of the calcium percarbonate, and part of it has been decomposed before combustion, thereby affecting the slagging rate; Example 29 prolongs the coating time, but the slagging rate is close to that of Example 20, indicating that the coating time of Example 20 is already the optimal time.

Claims

1. A high calorific value biomass fuel, characterized by: The specific preparation method is: (1) The straw was crushed using a pulverizer, and particles with a particle size of less than 3 mm were retained after screening. The particles were then placed in a de-impurity device to remove impurities to obtain particles a. Then, 20 parts of particles a and water were mixed at a solid-liquid ratio of 1:5-7 g / mL, and 0.3%-0.5% of the mass of particles a hydrolase was added at the same time. The reaction was carried out for 2-4 hours to obtain reactant a. (2) Adding reactant a into a fermentation tank, adding yeast of 0.2-0.4% by weight of particle a and 1-2 parts of fermentation accelerator, and performing anaerobic fermentation at 30-32° C. for 2-3 days. After the fermentation is completed, filtering to obtain solid a and filtrate a, drying the solid a, adding dicyclohexylcarbodiimide to the filtrate a, and filtering to obtain liquid a; (3) adding the dried solid a, liquid a and 1-2 parts of zinc trifluoromethanesulfonate into a reactor, and then reacting at 80-90° C. and 0.2-0.3 MPa for 2.5-3.5 hours to obtain product a after the reaction is completed; (4) First, 0.6-1 parts of urea-formaldehyde resin and 0.6% by weight of ammonium chloride are uniformly mixed, and then product a and 1-1.2 parts of anti-slagging agent are added and uniformly mixed, and then extruded at 50-55°C and 16-20MPa pressure to obtain biomass briquette fuel; Wherein, the preparation method of the fermentation accelerator is: Dissolve 3 parts of N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonic acid in 10 parts of water, then add sodium hydroxide solution to adjust the pH value to 6.5-6.7; Among them, urea-formaldehyde resin also includes the following processing methods: (1) Add 0.3-0.5% of the mass of perfluoropolyether-based surfactant to KH-560, and then add water to prepare a dilute solution with a concentration of 0.9-1.1% to obtain a modified solution; (2) polyoxyethylene hydrogenated castor oil and anhydrous ethanol are mixed in a volume ratio of 1:2.5-3.5 to obtain a coating solution, and then 6-10 μm wollastonite is immersed in the coating solution for 3-5 minutes, followed by drying to remove the anhydrous ethanol, and this cycle is repeated three times to obtain a modifier; (3) The urea-formaldehyde resin, the modifying liquid and the modifying agent are uniformly mixed in a mass ratio of 1:0.2~0.3:0.1~0.2 to obtain the modified urea-formaldehyde resin.

2. A high calorific value biomass fuel as claimed in claim 1, characterized in that: The preparation method of the anti-slagging agent is as follows: activated clay and calcium percarbonate are mixed in a mass ratio of 5:3 to obtain the anti-slagging agent.

3. A high calorific value biomass fuel as claimed in claim 2, characterized in that: The activated clay also includes the following treatment method: Activated clay and deionized water were mixed in a mass ratio of 1:8 and stirred to obtain a suspension, and then 0.7-0.8% of tetrabutylammonium hexafluorophosphate by mass of the activated clay was added, and the pH value was adjusted to 10.4-10.8 after stirring, and then the temperature was raised to 80-90°C for reaction for 3-4 hours. After the reaction was completed, the filter was filtered, and the filter cake was washed three times with anhydrous ethanol, and then dried and crushed to obtain the modified activated clay.

4. A high calorific value biomass fuel as claimed in claim 2, characterized in that: The calcium percarbonate also includes the following processing method: The coating liquid a is obtained by uniformly mixing hydrogenated rosin glycerol ester and acetone in a mass ratio of 1:1-2, and then the calcium percarbonate is immersed in the coating liquid a for 2-4 minutes, followed by drying at 24-26°C. This cycle is repeated three times to obtain the coated calcium percarbonate.

Citation Information

Patent Citations

  • Method for preparing ethyl levulinate from wood fiber biomass

    CN107266312A

  • Preparation method for low-ash high-combustion-value bio-fuel

    CN107474891A