Cellulose-polyacrylamide gel adsorbent as well as preparation method and application thereof
By freeze-swelling treatment of microcrystalline cellulose and polyacrylamide in urea and sodium hydroxide solvents and crosslinking with epoxychlorohydrin, a cellulose-polyacrylamide gel adsorbent with porous structure was prepared, and the fibers were solved The problem of limited capacity of chlorophyte gel adsorbent and single structure of polyacrylamide gel achieves efficient adsorption and stability improvement of methylene blue.
Patent Information
- Application Number
- CN202411408107.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-10
- Publication Date
- 2024-11-29
AI Technical Summary
The adsorption capacity of existing cellulose gel adsorbents is limited and difficult to effectively separate in water bodies. The polyacrylamide gel has a single structure and a low specific surface area, resulting in poor adsorption performance and it is difficult to efficiently remove methylene blue water pollutant.
Microcrystalline cellulose and polyacrylamide are used as raw materials, and cellulose-polyacrylamide gel adsorbent is prepared by cross-linking of epoxychlorohydrin to form a porous structure and a high specific surface area, combining urea and hydroxide Sodium solvents promote reactions and form a stable crosslinking network.
It significantly improves the adsorption capacity of methylene blue in the water environment, enhances the adsorption capacity and efficiency, and the cellulose-polyacrylamide gel adsorbent has good mechanical strength and stability, which is easy to recover and reuse.
Smart Images

Figure CN119034702A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hydrogel adsorbent preparation, and specifically relates to a cellulose-polyacrylamide gel adsorbent and a preparation method and application thereof. Background Art
[0002] With the population expansion and the acceleration of urbanization, the demand for water resources is increasing day by day. At the same time, the problem of water pollution is becoming increasingly serious and has become an ecological and environmental problem that needs to be solved urgently. One of the main difficulties in sewage treatment is how to effectively separate the dispersed particulate matter in sewage. These particles are often difficult to be effectively removed due to their solidification stability and sedimentation stability. Among them, methylene blue, as an alkaline cationic dye, is widely used in the fields of textiles, coloring, leather, and printing, but its toxicity is not optimistic. At present, the main methods for treating dye wastewater are chemical, biological and physical methods. Among them, physical methods include extraction, membrane separation and adsorption.
[0003] Among the main oil adsorbents, cellulose-based adsorbents have significant advantages over traditional adsorbents based on mineral or petroleum materials due to their biodegradability and applicability. Polyacrylamide gel is formed by the polymerization of polyacrylamide molecules in aqueous solution. It is a common gel material. Its molecular structure is rich in amide groups, which can form hydrogen bonds with water molecules, so it can form a stable gel state in water. In addition, polyacrylamide hydrogel can be degraded by biodegradation or physical methods to reduce pollution to the environment, and its synthetic monomer can be obtained from biomass resources, which is renewable and helps reduce production costs and resource consumption.
[0004] However, although the cellulose gel adsorbent and polyacrylamide hydrogel adsorbent prepared by the existing technical methods have good adsorption performance, the adsorption capacity of the cellulose gel adsorbent is limited and it is difficult to effectively separate it in the water body, resulting in inconvenience in recovery and treatment after adsorption; while the polyacrylamide gel adsorbent is limited in its adsorption efficiency due to its single structure, low specific surface area and disordered pore structure. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a cellulose-polyacrylamide gel adsorbent and a preparation method and application thereof. Microcrystalline cellulose and polyacrylamide are used as raw materials, and epichlorohydrin is introduced and then a sol-gel method is used to prepare the cellulose-polyacrylamide gel adsorbent. The cellulose-polyacrylamide gel adsorbent is obtained by the preparation method of the present invention. The cellulose-polyacrylamide gel adsorbent not only solves the problem that cellulose is limited in adsorption capacity as an adsorbent and is difficult to be effectively separated in water, but also overcomes the defects of poor adsorption performance caused by the single structure and low specific surface area of polyacrylamide gel and the disordered pore structure, thereby effectively improving the adsorption capacity of methylene blue in the water environment.
[0006] In order to achieve the above purpose, the technical solution adopted in this application is:
[0007] The first object of the present invention is to provide a method for preparing the above-mentioned cellulose-polyacrylamide gel adsorbent, comprising the following steps:
[0008] S1, adding microcrystalline cellulose and polyacrylamide to a solvent and mixing them, and then performing freeze swelling treatment to promote the dissolution of the microcrystalline cellulose and the polyacrylamide to obtain swollen cellulose and swollen polyacrylamide. The solvent is composed of an aqueous solution of urea and sodium hydroxide.
[0009] S2. Mixing the swollen cellulose and the swollen polyacrylamide with epichlorohydrin to obtain a cellulose-polyacrylamide homogeneous solution.
[0010] S3, subjecting the cellulose-polyacrylamide homogeneous solution to gelation treatment, so as to allow electrophilic substitution reaction between microcrystalline cellulose, polyacrylamide and epichlorohydrin to generate intermolecular forces, thereby obtaining cellulose-polyacrylamide gel.
[0011] S4. The cellulose-polyacrylamide gel is freeze-dried to maintain the porous structure of the cellulose-polyacrylamide gel and increase the specific surface area to obtain a cellulose-polyacrylamide gel adsorbent.
[0012] Preferably, the mass ratio of microcrystalline cellulose, polyacrylamide and epichlorohydrin is 4:4:1.75-2; when too much epichlorohydrin is added, the surface of the cellulose-polyacrylamide gel is too viscous and difficult to elute; if the addition amount is too low, the cross-linking effect cannot be achieved, and the cellulose-polyacrylamide gel cannot be formed or eluted.
[0013] Preferably, the mass concentration of urea in the solvent is 140 g / L to 148 g / L, and the mass concentration of sodium hydroxide is 80 g / L to 86 g / L.
[0014] Preferably, the freeze swelling treatment is carried out under the conditions of: freezing at -20°C to -50°C for 12h to 24h; low temperature can weaken the hydrogen bonds and van der Waals forces between microcrystalline cellulose and polyacrylamide molecules, making their crystalline structures unstable; at the same time, under low temperature conditions, the solubility of urea and sodium hydroxide in water increases, which helps the solvent system to better penetrate into the microcrystalline cellulose and polyacrylamide, accelerating the dissolution process.
[0015] Preferably, the gelation treatment is performed under the conditions of: standing at 50° C. to 55° C. for 3 h to 4 h.
[0016] Preferably, the freeze-drying treatment is carried out at -10°C to -20°C for 24h to 36h. Freeze-drying helps to maintain the porous structure of the cellulose-polyacrylamide gel and increase the specific surface area, while direct drying easily leads to the adhesion and collapse of the porous structure of the cellulose-polyacrylamide gel.
[0017] Preferably, before freeze-drying the cellulose-polyacrylamide gel, the cellulose-polyacrylamide gel is washed with water to neutrality to eliminate the interference of alkaline substances on the use of the cellulose-polyacrylamide gel adsorbent and facilitate better freeze-drying.
[0018] The second object of the present invention is to provide a cellulose-polyacrylamide gel adsorbent prepared by the above-mentioned preparation method of the cellulose-polyacrylamide gel adsorbent.
[0019] The third object of the present invention is to provide the use of the above cellulose-polyacrylamide gel adsorbent in the preparation of a methylene blue adsorbent for adsorbing water.
[0020] Preferably, the application method is: mixing the cellulose-polyacrylamide gel adsorbent with the methylene blue aqueous solution and then adsorbing; wherein the mass concentration ratio of the cellulose-polyacrylamide gel adsorbent to the methylene blue aqueous solution is 0.1g~0.3g:50mg / L~200mg / L.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention provides a method for preparing a cellulose-polyacrylamide gel adsorbent, wherein microcrystalline cellulose and polyacrylamide are added to a solvent composed of urea and sodium hydroxide, mixed, and then subjected to freeze swelling treatment to obtain swollen cellulose and swollen polyacrylamide; the swollen cellulose and swollen polyacrylamide are mixed with epichlorohydrin and then subjected to gelation treatment to obtain a cellulose-polyacrylamide gel; the cellulose-polyacrylamide gel is dried to obtain a cellulose-polyacrylamide gel adsorbent. This method not only solves the problems of limited adsorption capacity, inconvenient recycling and treatment of cellulose as an adsorbent, and difficulty in effective separation in water bodies, but also overcomes the defects of low specific surface area and poor adsorption performance of polyacrylamide gel due to disordered pore structure, thereby effectively improving the adsorption capacity of methylene blue in water environments.
[0023] Among them, the mixed solution of urea, sodium hydroxide and water is used as a solvent, which not only effectively promotes the uniform dispersion and dissolution of microcrystalline cellulose, polyacrylamide and epichlorohydrin in the solvent, but also ensures the uniformity and stability of microcrystalline cellulose, polyacrylamide, epichlorohydrin and the solvent system; microcrystalline cellulose and polyacrylamide are used as raw materials, and the natural pore structure of microcrystalline cellulose and the high molecular chain flexibility of polyacrylamide are successfully retained by freeze swelling treatment in the solvent of urea and sodium hydroxide aqueous solution; the epoxy group of epichlorohydrin has high reactivity, and under the catalysis of alkali, it can undergo electrophilic substitution reaction with the hydroxyl or amino group on the molecular chain of microcrystalline cellulose or polyacrylamide to generate a stable covalent bond cross-linked network, and urea can not only promote the swelling behavior of microcrystalline cellulose and polyacrylamide at low temperature, but also help to stabilize the pH value of the system, making the electrophilic substitution reaction more efficient. This cross-linked network structure not only enhances the overall stability and mechanical strength of the cellulose-polyacrylamide gel adsorbent, but also promotes the formation of a regular and continuous porous structure inside the cellulose-polyacrylamide gel adsorbent. The porous structure of the cellulose-polyacrylamide gel is retained through freezing treatment, and the specific surface area is increased, so that the prepared cellulose-polyacrylamide gel adsorbent has a higher adsorption capacity and better adsorption efficiency.
[0024] 2. The cellulose-polyacrylamide gel adsorbent prepared by the present invention has a three-dimensional network structure, which gives the cellulose-polyacrylamide gel adsorbent an excellent pore structure, a high specific surface area and abundant adsorption sites, thereby significantly enhancing the adsorption performance of the cellulose-polyacrylamide gel adsorbent. At the same time, the cellulose-polyacrylamide gel adsorbent also has good mechanical strength and stability, which is convenient for recycling and reuse in practical applications, reduces processing costs, and improves resource utilization.
[0025] Among them, the cellulose-polyacrylamide gel adsorbent of the present invention integrates multiple modes of action, including physical adsorption, chemical adsorption, and electrostatic action. First, its three-dimensional network structure not only provides more contact opportunities and adsorption paths for methylene blue molecules, but also greatly promotes the rapid penetration and diffusion of methylene blue molecules inside the cellulose-polyacrylamide gel adsorbent, ensuring the efficient capture and stable fixation of methylene blue molecules; secondly, the carboxyl functional groups on the microcrystalline cellulose molecular chain and the amide functional groups rich in polyacrylamide molecular chains, in the adsorption process, these functional groups can interact with the methylene blue molecules, and through the formation of hydrogen bonds and ionic bonds, the binding force between the cellulose-polyacrylamide gel adsorbent and the methylene blue molecules is significantly enhanced, and the firmness and selectivity of the adsorption are improved; in addition, the cellulose-polyacrylamide gel adsorbent of the present invention also has significant charge characteristics, and its surface charge can produce strong electrostatic attraction or repulsion with the charge of the methylene blue molecules. This mechanism of action further improves the efficiency of the adsorption process and ensures the efficient removal of the methylene blue molecules.
[0026] 3. The adsorption capacity of the cellulose-polyacrylamide gel adsorbent prepared by the present invention for methylene blue in water environment is the highest when 0.2 g of cellulose-polyacrylamide gel adsorbent is used and the mass concentration of the methylene blue aqueous solution is 150 g / mL.
[0027] 4. The preparation method of the cellulose-polyacrylamide gel adsorbent provided by the present invention has the advantages of easy raw material acquisition and low cost, simple synthesis steps, mild reaction conditions, and easy industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a product diagram of cellulose-polyacrylamide gel adsorbent prepared in Examples 1 to 4 and Comparative Examples 1 to 9.
[0029] Figure 2 This is the infrared spectrum of the cellulose-polyacrylamide gel adsorbent prepared in Example 3.
[0030] Figure 3 Surface scans of pure cellulose gel adsorbent, pure polyacrylamide gel adsorbent and cellulose-polyacrylamide gel adsorbent prepared in Example 3, wherein (a) is a surface scan of pure cellulose gel adsorbent, (b) is a surface scan of pure polyacrylamide gel adsorbent, and (c) is a surface scan of cellulose-polyacrylamide gel adsorbent prepared in Example 3.
[0031] Figure 4 This is the XRD spectrum of the cellulose-polyacrylamide gel adsorbent prepared in Example 3.
[0032] Figure 5This is a diagram showing the removal effects of the cellulose-polyacrylamide gel adsorbent prepared in Example 3 at different initial mass concentrations of pollutants.
[0033] Figure 6 This is a diagram showing the removal effects of different dosages of the cellulose-polyacrylamide gel adsorbent prepared in Example 3.
[0034] Figure 7 The kinetic fitting diagram of the adsorption of methylene blue by the cellulose-polyacrylamide gel adsorbent prepared in Example 3, wherein (a) is a pseudo-first-order kinetic model and (b) is a pseudo-second-order kinetic model.
[0035] Figure 8 This is a diagram showing the removal effect of pure cellulose gel adsorbent, pure polyacrylamide gel adsorbent and cellulose-polyacrylamide gel adsorbent of Example 3 on methylene blue. DETAILED DESCRIPTION
[0036] The technical solution of the present invention will be clearly and completely described below in combination with the data in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] The following experimental methods and detection methods, unless otherwise specified, are conventional methods; the following reagents and raw materials, unless otherwise specified, are commercially available reagents and raw materials. Urea, sodium hydroxide, microcrystalline cellulose, polyacrylamide, and N,N'-methylenebisacrylamide used in the present invention were all purchased from Shanghai MacLean Biochemical Technology Co., Ltd.; epichlorohydrin was purchased from Tianjin Damao Chemical Reagent Factory; and methylene blue was purchased from Tianjin Aopusheng Chemical Co., Ltd.
[0038] The instruments used in the present invention are an electronic balance of model GL124-1SCN produced by Sartorius Scientific Instruments Co., Ltd.; a precision profit-enhancing electric stirrer of model JJ-1 produced by Guohua Co., Ltd.; a circulating water multi-purpose vacuum pump of model SHB-Ⅲ produced by Zhengzhou Great Wall Science, Industry and Trade Co., Ltd.; a freeze dryer of model SCIENTZ-12N produced by Ningbo Xinzhi Biotechnology Co., Ltd.; a Fourier transform infrared spectrometer of model Nicolet iS50 produced by Thermo Fisher Scientific; a scanning electron microscope of model S-3400N produced by Hitachi Scientific Instruments Co., Ltd. of Japan; an X-ray diffractometer of model D2 Phaser produced by Bruker Corporation; and a double-beam ultraviolet-visible spectrophotometer of model TU-1901 produced by Beijing Puxi General Instrument Co., Ltd.
[0039] In the prior art, although cellulose and polyacrylamide each have application potential in the field of sewage treatment, they each have significant limitations. Although cellulose as an adsorbent is biodegradable and widely available, its adsorption capacity is limited, and it is easy to form agglomerates during the water treatment process, which makes recovery and treatment difficult, and also affects its effective separation in the water body. On the other hand, although polyacrylamide gel has good stability and plasticity, its single structural function, low specific surface area and complex pore structure limit the improvement of its adsorption performance, making it difficult to meet the needs of efficient removal of complex pollutants in sewage.
[0040] In view of the problems existing in the prior art, the present invention provides a preparation method of a cellulose-polyacrylamide gel adsorbent, comprising the following steps: adding microcrystalline cellulose and polyacrylamide into a solvent and mixing them, and then performing freeze swelling treatment to promote the dissolution of the microcrystalline cellulose and the polyacrylamide to obtain swollen cellulose and swollen polyacrylamide; wherein the solvent is composed of an aqueous solution of urea and sodium hydroxide; mixing the swollen cellulose and the swollen polyacrylamide with epichlorohydrin to obtain a cellulose-polyacrylamide homogeneous solution; performing gelation treatment on the cellulose-polyacrylamide homogeneous solution to allow electrophilic substitution reaction to occur between the microcrystalline cellulose, the polyacrylamide and the epichlorohydrin to generate intermolecular forces to obtain a cellulose-polyacrylamide gel; and performing freeze drying treatment on the cellulose-polyacrylamide gel to maintain the porous structure of the cellulose-polyacrylamide gel and increase the specific surface area to obtain the cellulose-polyacrylamide gel adsorbent.
[0041] The invention uses microcrystalline cellulose and polyacrylamide as raw materials, performs freeze swelling treatment in a solvent of urea and sodium hydroxide aqueous solution, and successfully retains the natural pore structure of microcrystalline cellulose and the high molecular chain flexibility of polyacrylamide; epichlorohydrin is used as a cross-linking agent, and plays a catalytic role under the alkaline condition of sodium hydroxide, and undergoes electrophilic substitution reaction with hydroxyl groups in microcrystalline cellulose and amide groups of polyacrylamide to form a covalent bond cross-linking network, and the cross-linking structure not only enhances the overall stability and mechanical strength of the cellulose-polyacrylamide gel adsorbent, but also promotes the formation of a regular and continuous porous structure inside the cellulose-polyacrylamide gel adsorbent; the porous structure of the cellulose-polyacrylamide gel is retained by the freezing treatment, and the specific surface area of the cellulose-polyacrylamide gel adsorbent is increased, so that the prepared cellulose-polyacrylamide gel adsorbent has a higher adsorption capacity and a more excellent adsorption efficiency. The cellulose-polyacrylamide gel adsorbent prepared by the method not only solves the problems of limited adsorption capacity, inconvenient recycling and treatment, and difficulty in effective separation in water bodies, but also overcomes the defects of poor adsorption performance caused by the single structure, low specific surface area, and disordered pore structure of polyacrylamide gel, thereby effectively improving the adsorption capacity of methylene blue in water environment.
[0042] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments:
[0043] Example 1
[0044] A method for preparing a cellulose-polyacrylamide gel adsorbent comprises the following steps:
[0045] S1. Use an electronic balance to accurately weigh 12 g of urea and 7 g of sodium hydroxide, place them in a 250 mL beaker, then add 81 mL of distilled water to the beaker to dissolve them, and use a glass rod to stir into a uniform solvent.
[0046] S2. Add 4 g of microcrystalline cellulose and 4 g of polyacrylamide to the solvent, stir thoroughly for 30 min, wrap it with plastic wrap and put it in a refrigerator at -20°C for 12 h to obtain swollen cellulose and swollen polyacrylamide.
[0047] S3. After freezing, thaw at room temperature first, then use an electric stirrer to stir thoroughly for 30 minutes. During the stirring process, add 2 g of epichlorohydrin to obtain a cellulose-polyacrylamide homogeneous solution, then pour it into a suction filtration bottle and filter it 5 times. After the filtration is completed, place it in a blast oven at 50°C for 4 hours to obtain a cellulose-polyacrylamide gel.
[0048] S4. After washing the cellulose-polyacrylamide gel with deionized water until it is neutral, the gel is placed in a refrigerator and frozen at -10°C for 24 hours to obtain a cellulose-polyacrylamide gel adsorbent, such as Figure 1 As shown in (a) in .
[0049] Example 2
[0050] A preparation method of a cellulose-polyacrylamide gel adsorbent is the same as the preparation method of Example 1, except that the gelation treatment temperature is 55° C., and comprises the following steps:
[0051] S1. Use an electronic balance to accurately weigh 12 g of urea and 7 g of sodium hydroxide, place them in a 250 mL beaker, then add 81 mL of distilled water to the beaker to dissolve them, and use a glass rod to stir into a uniform solvent.
[0052] S2. Add 4 g of microcrystalline cellulose and 4 g of polyacrylamide to the solvent, stir thoroughly for 30 min, wrap it with plastic wrap and put it in a refrigerator at -20°C for 12 h to obtain swollen cellulose and swollen polyacrylamide.
[0053] S3. After freezing, thaw at room temperature first, then use an electric stirrer to stir thoroughly for 30 minutes. During the stirring process, add 2 g of epichlorohydrin to obtain a cellulose-polyacrylamide homogeneous solution, then pour it into a suction filtration bottle and filter it 5 times. After the filtration is completed, place it in a forced air oven at 55°C for 4 hours to obtain a cellulose-polyacrylamide gel.
[0054] S4. After washing the cellulose-polyacrylamide gel with deionized water until it is neutral, the gel is placed in a refrigerator and frozen at -10°C for 24 hours to obtain a cellulose-polyacrylamide gel adsorbent, such as Figure 1 As shown in (b) in .
[0055] Example 3
[0056] A method for preparing a cellulose-polyacrylamide gel adsorbent is the same as the method of Example 1, except that the mass ratio of microcrystalline cellulose, polyacrylamide and epichlorohydrin is 4:4:1.75, and the gelation treatment time is 3 hours, comprising the following steps:
[0057] S1. Use an electronic balance to accurately weigh 12 g of urea and 7 g of sodium hydroxide, place them in a 250 mL beaker, then add 81 mL of distilled water to the beaker to dissolve them, and use a glass rod to stir into a uniform solvent.
[0058] S2. Add 4 g of microcrystalline cellulose and 4 g of polyacrylamide to the above solvent, stir thoroughly for 30 min, wrap it with plastic wrap and put it in a refrigerator at -20°C for 12 h to obtain swollen cellulose and swollen polyacrylamide.
[0059] S3. After freezing, thaw at room temperature first, then use an electric stirrer to stir thoroughly for 30 minutes. During the stirring process, add 1.75g of epichlorohydrin to obtain a cellulose-polyacrylamide homogeneous solution, then pour it into a suction filtration bottle and filter it 5 times. After the filtration is completed, place it in a blast oven at 50°C for 3 hours to obtain a cellulose-polyacrylamide gel.
[0060] S4. After washing the cellulose-polyacrylamide gel with deionized water until it is neutral, the gel is placed in a refrigerator and frozen at -10°C for 24 hours to obtain a cellulose-polyacrylamide gel adsorbent, such as Figure 1 As shown in (c) in .
[0061] Example 4
[0062] A method for preparing a cellulose-polyacrylamide gel adsorbent, which has the same preparation steps as those in Example 3, except that the gelation treatment temperature is 55° C., comprises the following steps:
[0063] S1. Use an electronic balance to accurately weigh 12 g of urea and 7 g of sodium hydroxide, place them in a 250 mL beaker, then add 81 mL of distilled water to the beaker to dissolve them, and use a glass rod to stir into a uniform solvent.
[0064] S2. Add 4 g of microcrystalline cellulose and 4 g of polyacrylamide to the solvent and stir thoroughly for 30 min. Add 1.75 g of epichlorohydrin during stirring to obtain a cellulose-polyacrylamide homogeneous solution. After stirring, wrap it with plastic wrap and put it in a refrigerator and freeze it at -20°C for 12 h to obtain swollen cellulose and swollen polyacrylamide.
[0065] S3. After freezing, thaw at room temperature first, then use an electric stirrer to fully stir for 30 minutes, pour into a suction filtration bottle and filter 5 times. After the filtration is completed, place it in a forced air oven at 55°C for 3 hours to obtain cellulose-polyacrylamide gel.
[0066] S4. After washing the cellulose-polyacrylamide gel with deionized water until it is neutral, the gel is placed in a refrigerator and frozen at -10°C for 24 hours to obtain a cellulose-polyacrylamide gel adsorbent, such as Figure 1 As shown in (d) in .
[0067] Example 5
[0068] A method for preparing a cellulose-polyacrylamide gel adsorbent has the same preparation steps as those of Example 4, except that the freezing temperature in step S2 is replaced from -20°C to -50°C, and the freezing time is replaced from 12h to 24h.
[0069] Example 6
[0070] A method for preparing a cellulose-polyacrylamide gel adsorbent has the same preparation steps as those of Example 4, except that in step S4, the freezing temperature is replaced from -10°C to -20°C, and the freezing time is replaced from 24h to 36h.
[0071] Example 7
[0072] A method for preparing a cellulose-polyacrylamide gel adsorbent has the same preparation steps as those of Example 1, except that in step S1, the mass of urea is replaced from 12 g to 11.34 g, and the mass of sodium hydroxide is replaced from 7 g to 6.48 g.
[0073] Comparative Example 1
[0074] A method for preparing a cellulose-polyacrylamide gel adsorbent is the same as the method of Example 1, except that the crosslinking agent is replaced by N,N'-methylenebisacrylamide instead of epichlorohydrin, and the mass ratio of microcrystalline cellulose, polyacrylamide and N,N'-methylenebisacrylamide is 3:3:1, comprising the following steps:
[0075] S1. Use an electronic balance to accurately weigh 12 g of urea and 7 g of sodium hydroxide, place them in a 250 mL beaker, then add 81 mL of distilled water to the beaker to dissolve them, and use a glass rod to stir into a uniform solvent.
[0076] S2. Add 3 g of microcrystalline cellulose and 3 g of polyacrylamide to the solvent, stir thoroughly for 30 min, wrap it with plastic wrap and put it in a refrigerator at -20°C for 12 h to obtain swollen cellulose and swollen polyacrylamide.
[0077] S3. After freezing, thaw at room temperature first, then use an electric stirrer to stir thoroughly for 30 minutes. During the stirring process, add 1g of N,N'-methylenebisacrylamide to obtain a cellulose-polyacrylamide homogeneous solution, then pour it into a suction filtration bottle and filter it 5 times. After the filtration is completed, place it in a forced air oven at 50°C for 4 hours to obtain a cellulose-polyacrylamide gel.
[0078] S4. Wash the cellulose-polyacrylamide gel with deionized water until it is neutral, and then freeze it in a refrigerator at -10°C for 24 hours to obtain a cellulose-polyacrylamide gel adsorbent.
[0079] Comparative Example 2
[0080] A method for preparing a cellulose-polyacrylamide gel adsorbent is the same as the preparation method of Comparative Example 1, except that the mass ratio of microcrystalline cellulose, polyacrylamide and N,N'-methylenebisacrylamide is 4:4:1.14, and the gelation treatment temperature is 55°C.
[0081] Comparative Example 3
[0082] A method for preparing a cellulose-polyacrylamide gel adsorbent is the same as the preparation method of Comparative Example 1, except that the mass ratio of microcrystalline cellulose, polyacrylamide and N,N'-methylenebisacrylamide is 4:2:1.
[0083] Comparative Example 4
[0084] A method for preparing a cellulose-polyacrylamide gel adsorbent is the same as the preparation method of Comparative Example 3, except that the mass ratio of microcrystalline cellulose, polyacrylamide and N,N'-methylenebisacrylamide is 4:2:1, the gelation treatment temperature is replaced from 50°C to 55°C, and the obtained cellulose-polyacrylamide gel adsorbent is not formed.
[0085] Comparative Example 5
[0086] A method for preparing a cellulose-polyacrylamide gel adsorbent is the same as the preparation method of Comparative Example 3, except that the gelation treatment temperature is replaced from 50° C. to 60° C., and the obtained cellulose-polyacrylamide gel adsorbent is not formed.
[0087] Comparative Example 6
[0088] A method for preparing a cellulose-polyacrylamide gel adsorbent is the same as the preparation method of Comparative Example 1, except that the mass ratio of microcrystalline cellulose, polyacrylamide and N,N'-methylenebisacrylamide is 5:1:2, the gelation treatment temperature is replaced from 50°C to 60°C, and the obtained cellulose-polyacrylamide gel adsorbent is not formed.
[0089] Comparative Example 7
[0090] A method for preparing a cellulose-polyacrylamide gel adsorbent has the same preparation steps as those in Example 1, except that the mass ratio of microcrystalline cellulose, polyacrylamide and epichlorohydrin is 4:4:3.
[0091] Comparative Example 8
[0092] A method for preparing a cellulose-polyacrylamide gel adsorbent has the same preparation steps as those in Example 1, except that the mass ratio of microcrystalline cellulose, polyacrylamide and epichlorohydrin is 4:4:1.5.
[0093] Although the cellulose-polyacrylamide gels of Comparative Examples 1 to 3 can be eluted and formed, after elution and freeze-drying, it is found that the surface of the cellulose-polyacrylamide gel is too soft and the effect is not ideal. Figure 1 As shown in (e), (f), and (g); the cellulose-polyacrylamide gel obtained in Comparative Examples 4 to 6 was not formed, as shown in Figure 1 As shown in (h), (i), and (j); Comparative Examples 7 to 8, the surface of the cellulose-polyacrylamide gel is too viscous and difficult to elute, such as Figure 1 (k) and (l) in .
[0094] Taking the cellulose-polyacrylamide gel prepared in Example 3 of the present invention as an example, it is applied to the adsorption of methylene blue in a water environment. The specific application method and results are shown below:
[0095] a. Testing and characterization of cellulose-polyacrylamide gel adsorbent:
[0096] Fourier transform infrared spectroscopy analysis: After the prepared cellulose / polyacrylamide gel adsorbent is freeze-dried, it is placed in an agate mortar and mixed with KBr to grind into a fine powder state, and then placed in a tablet press to press it into a light-transmitting thin sheet, and then placed in the sample analysis room for analysis and detection, and the scanning range is set to 4000cm -1 ~500cm -1 .
[0097] Scanning electron microscopy analysis: The prepared cellulose-polyacrylamide gel adsorbent was placed in a buffer solution until it reached a swelling equilibrium state, and then freeze-dried for one day. After freeze-drying, the gel adsorbent sample was broken by tweezers in a low-temperature environment of liquid nitrogen to obtain a cross-section sample. The broken sample was fixed on the conductive glue of the copper platform to ensure that the sample was stable and easy to observe. The sample surface was then ion sputtered and gold-plated, and placed in a sample chamber under vacuum conditions. The surface morphology of the cellulose-polyacrylamide gel adsorbent was scanned and observed using a scanning electron microscope to obtain detailed microstructural information.
[0098] X-ray diffraction analysis: Use an X-ray desktop diffractometer for analysis and detection. First set the state parameters: scanning voltage 220V, X-ray generation range 30KV / 10mA, scanning degree range -3°~160°. Take an appropriate amount of the prepared cellulose / polyacrylamide gel adsorbent sample, grind it into powder through fine rolling operation, and sieve it to ensure its particle size uniformity. Send the sieved powder into the sample pool, use vibration to make it slowly enter the channel, and adjust the vibration intensity to make the sample fully cover the sample pool. After filling about three-quarters of the capacity, start analysis and detection.
[0099] b. Test of the adsorption performance of cellulose-polyacrylamide gel adsorbent on methylene blue:
[0100] ① Weigh 0.1 g of the cellulose-polyacrylamide gel prepared in Example 3 and add it to an aqueous solution of methylene blue with an initial mass concentration of 50 mg / L, 75 mg / L, 100 mg / L, 150 mg / L, and 200 mg / L. After adsorption for 12 hours, the removal rate is calculated after the cellulose-polyacrylamide gel is adsorbed to equilibrium.
[0101] ② Weigh 0.1g, 0.15g, 0.2g, 0.25g and 0.3g of the cellulose-polyacrylamide gel of Example 3 and add them into a methylene blue aqueous solution with an initial mass concentration of 150mg / L, and calculate the removal rate after adsorption for 2h.
[0102] ③ Weigh 0.2 g of pure cellulose gel adsorbent, pure polyacrylamide gel adsorbent and cellulose-polyacrylamide gel adsorbent of Example 3 respectively, add them into a methylene blue aqueous solution with an initial mass concentration of 150 mg / L, and calculate the removal rate after adsorption for 2 hours.
[0103]
[0104] Where: c0 is the initial mass concentration of methylene blue aqueous solution, mg / L; c e is the mass concentration of methylene blue aqueous solution after adsorption, mg / L.
[0105] c. Adsorption kinetics
[0106] Weigh 0.2 g of completely dried cellulose-polyacrylamide gel adsorbent and add it to a methylene blue aqueous solution with an initial mass concentration of 150 mg / L to allow it to dynamically adsorb to an equilibrium state. Then calculate the adsorption amount q at different times, as shown in formula (2).
[0107] The calculation formulas of the first-order kinetic equation and the pseudo-second-order kinetic equation are shown in (3) and (4).
[0108]
[0109] ln(q e -q t )=ln q e -k1t (3)
[0110]
[0111] Where: V is the volume of heavy metal ion solution, mL; m is the amount of cellulose-polyacrylamide gel adsorbent, g; q t is the adsorption amount at time t, mg / g; q e is the equilibrium adsorption amount, mg / g; k1 is the pseudo-first-order kinetic adsorption rate constant; k2 is the pseudo-second-order kinetic adsorption rate constant; the kinetic model fitting parameters are shown in Table 1.
[0112] Infrared spectroscopy refers to the analysis and identification of material molecules using infrared spectroscopy. Figure 2 This is the infrared spectrum of the cellulose-polyacrylamide gel adsorbent prepared in Example 3. Figure 2 It is concluded that at 1450cm -1、3450cm -1 The peaks at 1579cm-1 are the stretching vibration absorption peaks of the methylene and hydroxyl groups of microcrystalline cellulose; -1 、3450cm -1 The peaks are the stretching vibration absorption peaks of the amide and amino groups of polyacrylamide. These characteristic absorption peaks can be found in the cellulose-polyacrylamide gel adsorbent, which means that the two raw materials can be well blended and formed, and the product is mainly composed of microcrystalline cellulose and polyacrylamide, which is consistent with the expected results.
[0113] Scanning electron microscopy works by emitting an electron beam that interacts with the sample surface, generating multiple signals that are then captured and interpreted to provide high-resolution surface topography information. Figure 3 Surface scans of pure cellulose gel adsorbent, pure polyacrylamide gel adsorbent and cellulose-polyacrylamide gel adsorbent prepared in Example 3, wherein (a) is a surface scan of pure cellulose gel adsorbent, (b) is a surface scan of pure polyacrylamide gel adsorbent, and (c) is a surface scan of cellulose-polyacrylamide gel adsorbent prepared in Example 3; Figure 3 (a)(b)(c) It is concluded that pure cellulose gel adsorbent exhibits low porosity characteristics, and its pore structure distribution is also uneven, which limits its adsorption efficiency. In contrast, the pore structure of pure polyacrylamide gel adsorbent is relatively simple and disordered, which also affects its adsorption efficiency in water treatment; while cellulose-polyacrylamide gel adsorbent is a porous material with obvious interconnected pores and folds, which can swell rapidly in water bodies and be used as an adsorption material. This also shows that the cellulose-polyacrylamide gel adsorbent can provide abundant adsorption sites for water treatment and effectively solve the problem of water pollution.
[0114] Figure 4 The XRD spectrum of the cellulose-polyacrylamide gel adsorbent prepared in Example 3; Figure 4 It can be analyzed that microcrystalline cellulose is a cellulose material with a crystalline structure, and polyacrylamide is a linear high molecular polymer with an amorphous structure. After the dissolution and gelation process, the crystal structure of the two finally changes from a crystalline state to an amorphous state. The synthesized cellulose-polyacrylamide gel adsorbent only shows a weak diffraction peak at around 20°, indicating that the cellulose-polyacrylamide gel adsorbent is mainly non-crystalline and contains a small amount of loosely structured crystals, and is an amorphous structural material.
[0115] Figure 5 The figure is a diagram showing the removal effect of the cellulose-polyacrylamide gel adsorbent prepared in Example 3 at different initial mass concentrations. Figure 5As shown in the figure, with the increase of the initial mass concentration of the solution, the removal rate of methylene blue by cellulose-polyacrylamide gel adsorbent shows an overall trend of first increasing and then decreasing. In particular, when the initial mass concentration of methylene blue in the solution is 150 mg / L, the removal rate of cellulose-polyacrylamide gel adsorbent reaches a peak value. At a lower initial mass concentration of methylene blue aqueous solution, the adsorption efficiency of cellulose-polyacrylamide gel adsorbent is relatively low due to the weak mass transfer driving force. With the increase of the initial mass concentration of methylene blue, the mass transfer driving force gradually increases, and the adsorption performance of cellulose-polyacrylamide gel adsorbent also increases, resulting in an enhanced removal rate of methylene blue. However, it is worth noting that the adsorption capacity of cellulose-polyacrylamide gel adsorbent is limited, so when the mass concentration of methylene blue aqueous solution increases further, the removal rate decreases.
[0116] Figure 6 The removal effect diagram of different dosages of cellulose-polyacrylamide gel adsorbent prepared in Example 3 is shown. Figure 6 As shown in the figure, with the increase of the dosage of cellulose-polyacrylamide gel adsorbent, its removal rate of methylene blue generally shows a process of first increasing and then decreasing, and the best removal effect occurs when the dosage of cellulose-polyacrylamide gel adsorbent is 0.2g. At the low dosage stage, the removal rate is relatively low because the number of effective adsorption sites on the cellulose-polyacrylamide gel adsorbent is limited; when the dosage of cellulose-polyacrylamide gel adsorbent is too high, the sites that are not bound to methylene blue will polymerize, and this polymerization behavior will reduce the effective adsorption vacancies, thereby reducing the removal rate.
[0117] Table 1 shows the kinetic model fitting parameters
[0118]
[0119] Figure 7 The kinetic fitting diagram of the adsorption of methylene blue by the cellulose-polyacrylamide gel adsorbent prepared in Example 3, wherein (a) is a pseudo-first-order kinetic model and (b) is a pseudo-second-order kinetic model. Figure 7 The regression coefficient R in (a) and (b) 2 It was concluded that the pseudo-second-order kinetic model had a higher degree of agreement with the adsorption of methylene blue by cellulose-polyacrylamide gel adsorbent (R 2 >0.99), and further comparison revealed that the theoretical equilibrium adsorption amount calculated by the pseudo-second-order kinetic equation was closer to the measured equilibrium adsorption amount. Therefore, it can be inferred that the adsorption process of methylene blue by the cellulose-polyacrylamide gel adsorbent is more consistent with the description of the pseudo-second-order kinetic equation and belongs to chemical adsorption.
[0120] Figure 8The removal effect of pure cellulose gel adsorbent, pure polyacrylamide gel adsorbent and cellulose-polyacrylamide gel adsorbent in Example 3 on methylene blue is shown in Figure 2. Figure 8 The results showed that the removal rate of methylene blue by pure cellulose gel adsorbent was 41%, the removal rate of methylene blue by pure polyacrylamide gel adsorbent was 54%, and the removal rate of methylene blue by cellulose-polyacrylamide gel adsorbent was 71%.
[0121] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0122] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for preparing a cellulose-polyacrylamide gel adsorbent, characterized in that: The following steps are involved: After adding microcrystalline cellulose and polyacrylamide into a solvent and mixing, a freeze swelling treatment is performed to promote the dissolution of the microcrystalline cellulose and the polyacrylamide to obtain swollen cellulose and swollen polyacrylamide; Wherein, the solvent is composed of an aqueous solution containing urea and sodium hydroxide; mixing the swollen cellulose and the swollen polyacrylamide with epichlorohydrin to obtain a cellulose-polyacrylamide homogeneous solution; The cellulose-polyacrylamide homogeneous solution is subjected to gelation treatment to allow microcrystalline cellulose, polyacrylamide and epichlorohydrin to undergo electrophilic substitution reaction to generate intermolecular forces, thereby obtaining a cellulose-polyacrylamide gel; The cellulose-polyacrylamide gel is freeze-dried to maintain the porous structure of the cellulose-polyacrylamide gel, thereby obtaining a cellulose-polyacrylamide gel adsorbent.
2. The method for preparing the cellulose-polyacrylamide gel adsorbent according to claim 1, characterized in that: The mass ratio of the microcrystalline cellulose, polyacrylamide and epichlorohydrin is 4:4:1.75-2.
3. The method for preparing the cellulose-polyacrylamide gel adsorbent according to claim 1, characterized in that: The mass concentration of urea in the solvent is 140 g / L to 148 g / L, and the mass concentration of sodium hydroxide is 80 g / L to 86 g / L.
4. The method for preparing the cellulose-polyacrylamide gel adsorbent according to claim 1, characterized in that: The freeze swelling treatment is carried out under the conditions of -20°C to -50°C for 12h to 24h.
5. The method for preparing the cellulose-polyacrylamide gel adsorbent according to claim 1, characterized in that: The gelation treatment conditions are: standing at 50° C. to 55° C. for 3 h to 4 h.
6. The method for preparing the cellulose-polyacrylamide gel adsorbent according to claim 1, characterized in that: The freeze-drying treatment conditions are: drying at -10°C to -20°C for 24h to 36h.
7. The method for preparing the cellulose-polyacrylamide gel adsorbent according to claim 1, characterized in that: Before freeze-drying the cellulose-polyacrylamide gel, the cellulose-polyacrylamide gel is washed with water until it is neutral.
8. A cellulose-polyacrylamide gel adsorbent obtained by the preparation method of the cellulose-polyacrylamide gel adsorbent according to any one of claims 1 to 7.
9. Use of the cellulose-polyacrylamide gel adsorbent according to claim 8 in preparing a methylene blue adsorbent.
10. Use of the cellulose-polyacrylamide gel adsorbent according to claim 9 in preparing a methylene blue adsorbent, characterized in that: The application method is: The cellulose-polyacrylamide gel adsorbent is mixed with a methylene blue aqueous solution for adsorption; The mass concentration ratio of the cellulose-polyacrylamide gel adsorbent to the methylene blue aqueous solution is 0.1 g to 0.3 g: 50 mg / L to 200 mg / L.