A high temperature stable A-site high configuration entropy filled tungsten bronze ceramic and preparation method thereof
By regulating the composition and structure of tungsten bronze ceramics, introducing high configuration entropy, high temperature stability A-position high configuration entropy full tungsten bronze ceramics are prepared, and the temperature of multi-layer ceramic capacitors in the prior art is solved under high temperature conditions. The problem of insufficient stability achieves high temperature stability with a dielectric constant change of less than 15% and good dielectric constant stability.
Patent Information
- Application Number
- CN202310767771.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-27
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-06-27
AI Technical Summary
The existing multi-layer ceramic capacitors have insufficient temperature stability under high temperature conditions, especially when the dielectric constant changes are greater than 15% at above 200°C, making it difficult to meet the requirements of modern electronics industry for high temperature applications.
By regulating the composition and structure of tungsten bronze ceramics, high configuration entropy is introduced, and A-position high configuration entropy is prepared. The chemical formula is Sr4.5Ca0.5RTi3Nb7O30, combining high entropy and tungsten bronze structures, a specific Sintering process and adhesives form ceramic materials with a single phase structure.
It realizes excellent temperature stability of ceramic materials under high temperature conditions, the temperature range of dielectric constant changes less than 15% exceeds 200℃, and shows good dielectric constant stability in high bias electric field, satisfying the use of capacitors at high temperatures. Requirements.
Smart Images

Figure CN116813340B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional ceramics and relates to an A-site high configuration entropy filled tungsten bronze ceramic with high temperature stability and a preparation method thereof. Background Art
[0002] Multilayer ceramic capacitors (MLCC) are composed of a layer of ceramic dielectric and a layer of internal electrode alternating back and forth, and then the end electrodes are sealed at both ends. It is a structure similar to multiple capacitors stacked in parallel. Due to its small size and high capacitance, it is the most important application form of ceramic capacitors today and is widely used in the modern electronics industry. Among them, the temperature stability of MLCC dielectric materials is a very important performance indicator. With the continuous expansion of applications, such as automotive ABS, aerospace and other fields, new requirements have been put forward for its temperature stability at high temperatures. At present, the mainstream system of MLCC is a binary or ternary system based on BaTiO3, but there are very few systems that meet the capacity change of less than 15% above 200°C. Therefore, it is of great significance to develop new dielectric materials that meet the temperature stability requirements of high temperatures.
[0003] Tungsten bronze is the second largest dielectric material besides perovskite. Tungsten bronze oxide is composed of 10 oxygen octahedrons connected at the top. There are 4 pentagonal channels, 2 quadrilateral channels and 4 triangular channels at the A position. The center of the oxygen octahedron is usually occupied by Ti, Nb, Ta ions, while the pentagonal channels are preferentially occupied by large ions such as Ba and Sr. The quadrilateral channels are usually occupied by the second largest ions, such as rare earth elements such as La and Nd. The triangular channels are usually vacant and can also be occupied by small ions such as Li and Na. When all polygonal channels are occupied by ions, it is called a fully filled tungsten bronze structure, and its general structural formula can be written as [(A1)2(A2)4C4][(B1)2(B2)8]O 30 When the A1 and A2 positions are fully filled and the C position is vacant, it is called a full-type tungsten bronze structure, and the general formula is [(A1)2(A2)4][(B1)2(B2)8]O 30 When the A1 and A2 positions are partially filled and the C position is vacant, it is called an unfilled tungsten bronze structure, and its general formula is (A2, A1) B2O6.
[0004] In a thermodynamic system, entropy is a measure of the degree of disorder of the system. The higher the degree of disorder of the system, the greater the entropy. According to the Gibbs free energy formula, the Gibbs free energy of the system can be reduced by increasing the configuration entropy (Sconfig) of the system, thereby stabilizing the single-phase crystal structure. The concept of high entropy is widely used in alloys. High entropy alloys have attracted widespread attention from the scientific community for their excellent mechanical properties, corrosion resistance, and excellent thermal stability. However, the application of high entropy in the field of ceramics is relatively rare, and most of them are concentrated in the field of perovskites, while the application of high entropy in tungsten bronze structures is rarely reported. However, the tungsten bronze structure has a large degree of freedom in composition design, and it becomes easier to improve its performance through entropy engineering, which has broad development prospects. Summary of the invention
[0005] The purpose of the present invention is to provide a tungsten bronze ceramic with high temperature stability and high configuration entropy filling at the A site and a preparation method thereof in view of the deficiencies in the prior art. The present invention introduces high entropy into the tungsten bronze ceramic by regulating the composition and structure of the tungsten bronze components, so that the ceramic has excellent temperature stability.
[0006] In the first aspect, the present invention provides a high temperature stability A-site high configuration entropy filled tungsten bronze ceramic, the chemical formula of the ceramic is Sr 4.5 Ca 0.5 RTi3Nb7O 30 , and preferably R=La 0.5 Nd 0.5 ,La 1 / 3 Nd 1 / 3 Sm 1 / 3 ,La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 , and its corresponding A-site configuration entropy ΔS config They are 1.39R, 1.59R and 1.73R respectively.
[0007] In a second aspect, the present invention provides a method for preparing an A-site high configuration entropy filled tungsten bronze ceramic with high temperature stability, comprising:
[0008] (1) The raw materials SrCO3, CaCO3, La2O3, Nd2O3, Sm2O3, Eu2O3, TiO2 and Nb2O5 are prepared according to the chemical formula Sr 4.5 Ca 0.5 RTi3Nb7O 30 Mix the ingredients, ball grind until mixed evenly, then dry and sieve.
[0009] (2) The powder obtained in step (1) is calcined, ball-milled until mixed evenly, and then dried and sieved.
[0010] (3) Adding a binder to the powder obtained in step (2) to form a tablet, and then sintering the tablet to obtain a ceramic sheet.
[0011] Furthermore, in step (1), the ball milling medium is deionized water, and the ball milling time is 24 hours.
[0012] Furthermore, in step (2), the calcination temperature is 1200-1300° C., and the calcination time is 3-4 hours, preferably 1250° C., and the calcination time is 3 hours.
[0013] Furthermore, in step (3), the adhesive is a polyvinyl alcohol aqueous solution with a concentration of 5-10%, preferably 8 wt%, and the temperature of the plastic discharge is 600°C and the time is 2 hours.
[0014] Furthermore, in step (3), the sintering temperature is 1300-1350° C., the time is 3-4 hours, preferably 1325° C., the time is 3 hours, and the heating rate is 2° C. / min.
[0015] On the other hand, the present invention provides a tungsten bronze structural ceramic, including the above-mentioned high temperature stability A-site high configuration entropy filled tungsten bronze ceramic
[0016] The present invention combines high entropy with tungsten bronze structure, and the obtained A-site high configuration entropy filled tungsten bronze ceramic has a single-phase structure and excellent temperature stability, based on room temperature, especially when R=La 1 / 3 Nd 1 / 3 Sm 1 / 3 and La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 When the dielectric constant change value is less than 15%, the maximum temperature corresponding to the temperature range exceeds 200°C, which meets the high temperature use requirements of the capacitor and also shows excellent dielectric constant stability under high bias electric field. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 The X-ray diffraction pattern of the A-site high configuration entropy filled tungsten bronze ceramic material with high temperature stability of Example 1;
[0018] Figure 2 The surface microscopic morphology of the A-site high configuration entropy filled tungsten bronze ceramic material with high temperature stability of Example 1: (a) R = La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 ; (b) R = La 1 / 3 Nd 1 / 3 Sm 1 / 3 ; (c) R = La0.5 Nd 0.5 ;
[0019] Figure 3 The change of dielectric constant with temperature at different frequencies and temperature stability of the A-site high configuration entropy filled tungsten bronze ceramic material with high temperature stability of Example 1: (a) R = La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 ; (b) R = La 1 / 3 Nd 1 / 3Sm 1 / 3 ; (c) R = La 0.5 Nd 0.5 ; (d): The rate of change of dielectric constant with temperature, based on the room temperature dielectric constant;
[0020] Figure 4 The graph of the dielectric constant of the A-site high configuration entropy filled tungsten bronze ceramic material with high temperature stability of Example 1 as a function of the bias electric field at different temperatures: (a) R = La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 ; (b) R = La 1 / 3 Nd 1 / 3 Sm 1 / 3 ; (c) R = La 0.5 Nd 0.5 ; DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention.
[0022] Example 1
[0023] (1) Using CaCO3 (99.99%), SrCO3 (99.95%), TiO2 (99.99%), La2O3 (99.99%), Nd2O3 (99.99%), Sm2O3 (99.99%), Eu2O3 (99.99%), and Nb2O5 (99.99%) powders as raw materials, the raw material powders were mixed and weighed according to the corresponding stoichiometric ratio; the chemical formula is Sr 4.5 Ca 0.5 RTi3Nb7O 30 , R corresponds to La 0.5 Nd 0.5 ,La1 / 3 Nd 1 / 3Sm 1 / 3 ,La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 .
[0024] (2) According to the formula Where R is the ideal gas constant, x i is the molar concentration of each component in the same position, N is the number of components, and Sr is calculated. 4.5 Ca 0.5 RTi3Nb7O 30 In ceramics, R corresponds to La 0.5 Nd 0.5 ,La 1 / 3 Nd 1 / 3 Sm 1 / 3 ,La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 The configuration entropies are 1.39R, 1.59R and 1.73R respectively.
[0025] (3) The weighed raw materials were placed in a ball mill, and ball milled with ZrO2 balls using deionized water as the medium for 24 hours, and then placed in an oven at 80°C for drying. After drying, the ZrO2 balls and the powder were separated, and then the powder was sieved through a 120-mesh sieve;
[0026] (4) Pour the sieved powder into a crucible and pre-calculate it in air at 1250°C for 3 hours to obtain the desired target product. Then, the calcined powder is ball-milled again for 24 hours and passed through a 120-mesh sieve after grinding.
[0027] (5) adding 8 wt % of polyvinyl alcohol as a binder to the obtained mixed powder, grinding it and passing it through a 40-mesh sieve, pressing it into a disc with a diameter of 12 mm and a thickness of about 1.5 mm under a pressure of 100 MPa, and then extruding it at 600° C. for 3 hours;
[0028] (6) The molded body is sintered in an air atmosphere at 1325° C. for 3 hours, and taken out after natural cooling to obtain the A-site high configuration entropy filled tungsten bronze ceramic with the required high temperature stability.
[0029] The prepared A-site high configuration entropy filled tungsten bronze ceramic material with high temperature stability was subjected to X-ray diffraction analysis test. Figure 1 The X-ray diffraction patterns of the three samples obtained in Example 1 are shown.
[0030] The ceramic surface was treated and then analyzed by scanning electron microscope. Figure 2 The surface morphology of Example 1 is shown.
[0031] The ceramic surface was ground, thinned, polished, and then silver-plated for electrical performance testing. Figure 3 The dielectric temperature spectrum and temperature stability of Example 1 are shown; Figure 4 The variation of dielectric constant with bias electric field at different temperatures is shown.
[0032] Attached Figure 1 The X-ray diffraction diagram of Example 1 is shown. It can be seen from the diagram that the ceramic of Example 1 has no impurity phase, is basically consistent with the standard PDF card #00-059-0421, and has a space group of P4bm, which is a tetragonal tungsten bronze crystal system.
[0033] Attached Figure 2 The surface morphology of Example 1 is shown, from which it can be seen that the ceramic surface is dense.
[0034] Attached Figure 3 The dielectric temperature spectrum and temperature stability of Example 1 are shown. It can be seen from the figure that based on the room temperature dielectric constant, R = La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 and R=La 1 / 3 Nd 1 / 3 Sm 1 / 3 The dielectric constant change rate of the corresponding samples is less than ±15% when the temperature exceeds 200°C.
[0035] Attached Figure 4 The figure shows the change of dielectric constant with bias electric field at different temperatures. It can be seen from the figure that the dielectric constant begins to decrease with the increase of electric field, but its change value is small at different temperatures measured, which shows good voltage resistance.
[0036] The evaluation standard for the temperature stability of the dielectric constant of XNR ceramic capacitors is based on the room temperature dielectric constant (ε r (RT)) as the reference, the dielectric constant change rate is less than ±15%. Sr 4.5 Ca 0.5 RTi3Nb7O 30 The temperature stability of the ceramic dielectric constant is shown in Table 1. As the A-site configuration entropy increases, the temperature range that meets the standard gradually increases, especially at the high temperature end. 1 / 3 Nd 1 / 3Sm 1 / 3 and La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 When the temperature is higher than 200℃, the high temperature end exceeds 200℃. 4.5 Ca 0.5RTi3Nb7O 30 The temperature stability of ceramic dielectric constant plays a key role in regulating it to high temperature range.
[0037] Table 1 Sr 4.5 Ca 0.5 RTi3Nb7O 30 Ceramic dielectric properties parameters
[0038] R <![CDATA[ΔS config ]]> <![CDATA[ε r (RT)]]> Temperature range (℃) La 0 804 -60~57 <![CDATA[La 0.5 Nd 0.5 ]]> 1.39R 634 -30~152 <![CDATA[La 1 / 3 Nd 1 / 3 Sm 1 / 3 ]]> 1.59R 580 -4~242 <![CDATA[La 0.25 Nd 0.25 Sm 0.25 I 0.25 ]]> 1.73R 452 -12~278
[0039] The above contents are further detailed descriptions of the present invention in combination with specific embodiments. It cannot be determined that the specific implementation measures of the present invention are limited to these descriptions. Some non-essential improvements and adjustments made by technicians in this field based on the above contents of the present invention all belong to the protection content of the present invention.
Claims
1. A high temperature stable A-site high configuration entropy filled tungsten bronze ceramic, characterized by: The chemical formula of the ceramic is Sr 4.5 Ca 0.5 R Ti3Nb7O 30 ;in R =La 0.5 Nd 0.5 ,La 1 / 3 Nd 1 / 3 Sm 1 / 3 or La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 ;correspond R La 0.5 Nd 0.5 ,La 1 / 3 Nd 1 / 3 Sm 1 / 3 ,La 0.25 Nd 0.25 Sm 0.25 Eu 0.25 When the A-site configuration entropy of the ceramic is S config They are 1.39R, 1.59R and 1.73R respectively.
2. A method for preparing the A-site high configuration entropy filled tungsten bronze ceramic with high temperature stability as claimed in claim 1, characterized in that: The following steps are involved: (1) The raw materials SrCO3, CaCO3, La2O3, Nd2O3, Sm2O3, Eu2O3, TiO2 and Nb2O5 are prepared according to the chemical formula Sr 4.5 Ca 0.5 R Ti3Nb7O 30 Ingredients, ball-mill until mixed evenly, then dry and sieve; (2) calcining and ball-milling the powder obtained in step (1) until the mixture is uniformly mixed, drying and sieving; (3) The powder obtained in step (2) is added with a binder, pressed, molded, and then sintered to obtain the ceramic.
3. The preparation method according to claim 2, characterized in that: In step (1), the ball milling medium is deionized water.
4. The preparation method according to claim 2, characterized in that: In step (2), the calcination temperature is 1200° C. to 1300° C., and the calcination time is 3 to 4 hours.
5. The preparation method according to claim 2, characterized in that: In step (3), the adhesive is a polyvinyl alcohol aqueous solution with a concentration of 5-10 wt%, and the molding temperature is 600° C. for 3 hours.
6. The preparation method according to claim 2, characterized in that: In step (3), the sintering temperature is 1300-1350°C, the sintering time is 3-4 hours, and the heating rate is 2°C / min.
7. A capacitor, characterized in that: The invention comprises the A-site high configuration entropy filled tungsten bronze ceramic with high temperature stability as claimed in claim 1.