A method for preparing thermal insulation hollow blocks with recycled aggregate
By using fly ash, silicate cement and other materials to prepare recycled aggregate blocks and injecting foamed materials into the cavity, the problems of environmental pollution and insufficient insulation performance in construction waste treatment and recycling are solved, and the problem of Recycled aggregate blocks with low cost, high strength and good thermal insulation effect.
Patent Information
- Application Number
- CN202310687752.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-12
AI Technical Summary
In the prior art, the treatment and recycling of construction waste have problems of environmental pollution and resource waste, and the thermal insulation performance of recycled aggregates is insufficient, making it difficult to meet the needs of construction projects.
Use fly ash, silicate cement, recycled coarse aggregate, gravel, recycled fine aggregate, natural river sand, hydrated sodium silicate, straw fiber, aerogel and other materials to prepare insulation by stirring and vibration pressurization Hollow blocks and foamed materials are injected into the cavity to improve insulation performance.
Recycled aggregate blocks with low cost, high strength and good insulation effect are achieved, reducing energy consumption and carbon emissions, effectively making use of construction waste, and improving the toughness and insulation performance of the blocks.
Smart Images

Figure BDA0004278938990000071 
Figure BDA0004278938990000081 
Figure BDA0004278938990000091
Abstract
Description
Technical Field
[0001] The invention belongs to the field of building material preparation, and in particular relates to a method for preparing a heat-insulating hollow building block by using recycled aggregate. Background Art
[0002] With the increasing number of infrastructure construction in my country, a large amount of waste is generated during the laying, construction, and demolition of buildings. These wastes are usually mixed with a variety of materials, including discarded concrete, mortar, bricks, and wood. If these construction wastes are landfilled around the city or piled up in the suburbs without any treatment, it will not only pollute the environment, but also affect the appearance of the city. In order to effectively utilize construction waste and prevent environmental pollution and waste of resources, recycled concrete came into being. This kind of concrete is made from discarded concrete, mortar, bricks, and other raw materials in construction waste through a series of treatments. During the production process, compared with silicate cement concrete, it can reduce more than 70% of energy consumption and carbon emissions. This new preparation method can effectively utilize urban waste and avoid polluting the environment and wasting resources.
[0003] In order to improve the utilization of recycled aggregates and enhance the effect of construction, there are many related papers and patents. For example, Publication No. CN202010576626.2 "A method for preparing a recycled aggregate thermal insulation block" discloses a method for processing recycled coarse aggregates, which improves the tensile and compressive strength of the blocks by adding polyester fibers. Publication No. CN202210132287.8 "A recycled aggregate self-insulating block and its preparation method" discloses a recycled aggregate self-insulating block and its preparation method, focusing on using a new thermal insulation structure to enhance the thermal insulation performance of the block. Summary of the invention
[0004] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0005] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.
[0006] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a thermal insulation hollow block using recycled aggregate.
[0007] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing heat-insulating hollow blocks with recycled aggregates, comprising:
[0008] Prepare the raw materials for the base material of the thermal insulation hollow block: according to the components by weight, 130-210 parts of fly ash, 210-290 parts of silicate cement, 460-570 parts of recycled coarse aggregate, 570-690 parts of gravel, 310-370 parts of recycled fine aggregate, 250-310 parts of natural river sand, 50-110 parts of hydrated sodium silicate, 30-90 parts of straw fiber, 20-40 parts of metallurgical slag, 70-130 parts of aerogel, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water;
[0009] Preparation of block base material: Put recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and mix them evenly, then pour fly ash and silicate cement into the mixer and mix them, then add natural river sand, gravel, straw fiber, air entraining agent, water reducing agent, water and aerogel in sequence, mix and stir evenly to obtain the block base material;
[0010] Preparation of hollow blocks: Pressing the block base material into hollow blocks by a vibration pressurizing molding machine;
[0011] Preparation of heat-insulating hollow blocks: injecting the foaming material stock solution into the cavity of the hollow block, accounting for 40% to 60% of the volume of the cavity, and obtaining the heat-insulating hollow block after standing and curing.
[0012] As a preferred embodiment of the method of the present invention, the fly ash has a calcium oxide content greater than 15%.
[0013] As a preferred embodiment of the method of the present invention, the particle size of the recycled coarse aggregate is 4.75 mm to 10.0 mm, and the apparent density is 2050 to 2070 kg / m 3 The water absorption rate is 9.6~9.7%.
[0014] As a preferred embodiment of the method of the present invention, the particle size of the recycled fine aggregate is less than 4.75 mm, and the apparent density is 2310-2350 kg / m 3 The water absorption rate is 9.5~9.6%.
[0015] As a preferred embodiment of the method of the present invention, the natural river sand is medium sand with a fineness modulus of 2.3 to 3.0 and an average particle size of 0.5 mm to 0.3 mm.
[0016] As a preferred embodiment of the method of the present invention, the unfoamed thermal insulation material stock solution is prepared according to the following weight parts: 50-70 parts of phosphogypsum, 20-50 parts of fly ash, 5-10 parts of lime, 4-9 parts of hydrogen peroxide, 1-2 parts of foam stabilizer, 5-15 parts of silicon aerogel particles, and 20-60 parts of water.
[0017] As a preferred embodiment of the method of the present invention, the foamed thermal insulation material is in liquid state before foaming, which is called unfoamed thermal insulation material stock solution, and its preparation method includes:
[0018] The phosphogypsum is heated and fried at 170°C to obtain β-type hemihydrate phosphogypsum;
[0019] Then, fly ash, lime and silicon aerogel particles are added thereto and mixed to obtain a mixture;
[0020] Add hydrogen peroxide and foam stabilizer into warm water at 60-70°C, then pour water into the mixture and stir for 10-30 seconds to obtain the unfoamed thermal insulation material stock solution.
[0021] Another object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a thermal insulation hollow block using recycled aggregate to obtain a thermal insulation hollow block product.
[0022] Beneficial effects of the present invention:
[0023] (1) The present invention provides a method for preparing a recycled aggregate thermal insulation building block with low manufacturing cost. The method uses recycled aggregate to replace the coarse and fine aggregates in traditional concrete, crushes the recycled concrete building blocks into appropriate sizes, and adds hydrated sodium silicate, straw fiber, metallurgical slag, and aerogel materials. The synergistic effect of the raw materials makes the building blocks stronger, tougher, and more thermally insulating than traditional building blocks, so as to prepare thermal insulation hollow building blocks that meet engineering requirements.
[0024] (2) The present invention can not only solve the various problems caused by the rapid increase of construction waste in existing practice to the environment and resources, but also can reuse concrete block brick materials, turning waste into treasure and improving the thermal insulation of the original blocks. DETAILED DESCRIPTION
[0025] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0026] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0027] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0028] In the embodiment of the present invention, the particle size of the recycled coarse aggregate is 4.75 mm to 10.0 mm, and the apparent density is 2050 to 2070 kg / m 3 , water absorption rate is 9.6-9.7%; the particle size of recycled fine aggregate is <4.75mm, and the apparent density is 2310-2350kg / m 3 , water absorption rate is 9.5-9.6%; natural river sand is medium sand, its fineness modulus is 2.3-3.0, and the average particle size is 0.5mm-0.3mm, all of which are common commercial products;
[0029] In the embodiment of the present invention, the stone particle size is controlled at 15-4.7 mm, which is a common commercial product; the hydrated sodium silicate is derived from Jiashan Yourui Refractory Material Co., Ltd., model SP38, with a modulus of 3.30, a silicon dioxide concentration of 27.3%, and a sodium oxide concentration of 8.54%, which is a common commercial product; the straw fiber particle size is 50-150 mesh; the aerogel is derived from the product produced by A.B.A. and is a common commercial product; the air entraining agent in the present invention is derived from the α-olefin sodium sulfonate powder of China Light Industry Co., Ltd., with an active matter content of 92%, which is a common commercial product; the water reducer is derived from the high-performance standard water reducer of Hunan Zhongyan Building Technology Co., Ltd., model ZY-HPWR-S, which is a common commercial product; the foam stabilizer is derived from Ruiyuan Building Materials Chemical, which is a common commercial product; the silicon aerogel particles are derived from the products produced by A.B.A. and are common commercial products.
[0030] The unfoamed thermal insulation material stock solution of the present invention is prepared according to the following weight parts: 50-70 parts of phosphogypsum, 20-50 parts of fly ash, 5-10 parts of lime, 4-9 parts of hydrogen peroxide, 1-2 parts of foam stabilizer, 5-15 parts of silicon aerogel particles, and 20-60 parts of water. The preparation method thereof comprises:
[0031] The phosphogypsum is heated and fried at 170°C to obtain β-type hemihydrate phosphogypsum;
[0032] Then, fly ash, lime and silicon aerogel particles are added thereto and mixed to obtain a mixture;
[0033] Add hydrogen peroxide and foam stabilizer into warm water at 60-70°C, then pour water into the mixture and stir for 10-30 seconds to obtain the unfoamed thermal insulation material stock solution.
[0034] Example 1
[0035] The components of the heat-insulating hollow building blocks in this embodiment are as follows by weight:
[0036] 170 parts of fly ash, 270 parts of Portland cement, 430 parts of recycled coarse aggregate, 570 parts of gravel, 340 parts of recycled fine aggregate, 270 parts of natural river sand, 80 parts of hydrated sodium silicate, 50 parts of straw fiber, 30 parts of metallurgical slag, 90 parts of aerogel, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water.
[0037] The particle size of recycled coarse aggregate is 4.75mm~10.00mm, and the apparent density is 2050~2070kg / m 3 , water absorption rate is 9.6-9.7%; the particle size of recycled fine aggregate is <4.75mm, and the apparent density is 2310-2350kg / m 3 ; Natural river sand is medium sand with a fineness modulus of 2.3 to 3.0 and an average particle size of 0.5 mm to 0.3 mm.
[0038] The preparation method of the thermal insulation hollow block is as follows:
[0039] Put the recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and stir, then pour in fly ash and silicate cement and mix, then add natural river sand, gravel, straw fiber, air entraining agent, water reducing agent, water and aerogel in sequence, and then mix and stir to obtain the block base material.
[0040] The block base material is pressed into hollow blocks by a vibration press molding machine.
[0041] The foaming material is injected into the cavity of the hollow building block, and then the heat-insulating hollow building block is obtained after standing and curing.
[0042] Example 2
[0043] The components of the heat-insulating hollow building blocks in this embodiment are as follows by weight:
[0044] 170 parts of fly ash, 270 parts of Portland cement, 430 parts of recycled coarse aggregate, 570 parts of gravel, 340 parts of recycled fine aggregate, 270 parts of natural river sand, 80 parts of hydrated sodium silicate, 50 parts of straw fiber, 30 parts of metallurgical slag, 105 parts of aerogel, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water.
[0045] The particle size of recycled coarse aggregate is 4.75mm~10.00mm, and the apparent density is 2050~2070kg / m 3 , water absorption rate is 9.6-9.7%; the particle size of recycled fine aggregate is <4.75mm, and the apparent density is 2310-2350kg / m 3 ; Natural river sand is medium sand with a fineness modulus of 2.3 to 3.0 and an average particle size of 0.5 mm to 0.3 mm.
[0046] The preparation method of the heat-insulating hollow building block of this method is as follows:
[0047] Put the recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and stir, then pour in fly ash and silicate cement and mix, then add natural river sand, gravel, straw fiber, air entraining agent, water reducing agent, water and aerogel in sequence, and then mix and stir to obtain the block base material.
[0048] The block base material is pressed into hollow blocks by a vibration press molding machine.
[0049] The foaming material is injected into the cavity of the hollow building block, and then the heat-insulating hollow building block is obtained after standing and curing.
[0050] Example 3
[0051] The components of the heat-insulating hollow building blocks in this embodiment are as follows by weight:
[0052] 170 parts of fly ash, 270 parts of Portland cement, 430 parts of recycled coarse aggregate, 570 parts of gravel, 340 parts of recycled fine aggregate, 270 parts of natural river sand, 60 parts of hydrated sodium silicate, 50 parts of straw fiber, 30 parts of metallurgical slag, 90 parts of aerogel, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water.
[0053] The particle size of recycled coarse aggregate is 4.75mm~10.00mm, and the apparent density is 2050~2070kg / m 3 , water absorption rate is 9.6-9.7%; the particle size of recycled fine aggregate is <4.75mm, and the apparent density is 2310-2350kg / m 3 ; Natural river sand is medium sand with a fineness modulus of 2.3 to 3.0 and an average particle size of 0.5 mm to 0.3 mm.
[0054] The preparation method of the heat-insulating hollow building block of this method is as follows:
[0055] Put the recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and stir, then pour in fly ash and silicate cement and mix, then add natural river sand, gravel, straw fiber, air entraining agent, water reducing agent, water, aerogel in turn, and then mix and stir to obtain the block base material.
[0056] The block base material is pressed into a hollow block by a vibration pressure forming machine, the foaming material is injected into the cavity of the hollow block, and then the heat-insulating hollow block is obtained after standing and curing.
[0057] Comparative Example 1
[0058] The components of the heat-insulating hollow building blocks in this comparative example are as follows by weight:
[0059] 170 parts of fly ash, 270 parts of Portland cement, 430 parts of recycled coarse aggregate, 570 parts of gravel, 340 parts of recycled fine aggregate, 270 parts of natural river sand, 30 parts of metallurgical slag, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water.
[0060] The particle size of recycled coarse aggregate is 4.75mm~10.00mm, the apparent density is 2050~2070kg / m3, and the water absorption rate is 9.6~9.7%; the particle size of recycled fine aggregate is <4.75mm, the apparent density is 2310~2350kg / m3; natural river sand is medium sand, the fineness modulus is 2.3~3.0, and the average particle size is 0.5mm~0.3mm.
[0061] The preparation method of the heat-insulating hollow building block of this method is as follows:
[0062] Put the recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and stir, then pour in fly ash and silicate cement and mix and stir, then add natural river sand, gravel, straw fiber, aerogel, air entraining agent and water reducing agent in turn and mix and stir to obtain the block base material. The block base material is pressed into a hollow block by a vibration pressure molding machine. The foaming material is injected into the cavity of the hollow block, and then after standing and curing, the heat-insulating hollow block is obtained.
[0063] Comparative Example 2
[0064] The components of the thermal insulation hollow blocks in this example are as follows by weight:
[0065] 170 parts of fly ash, 270 parts of Portland cement, 430 parts of recycled coarse aggregate, 570 parts of gravel, 340 parts of recycled fine aggregate, 270 parts of natural river sand, 90 parts of hydrated sodium silicate, 50 parts of straw fiber, 30 parts of metallurgical slag, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water.
[0066] The particle size of recycled coarse aggregate is 4.75mm~10.00mm, the apparent density is 2050~2070kg / m3, and the water absorption rate is 9.6~9.7%; the particle size of recycled fine aggregate is <4.75mm, the apparent density is 2310~2350kg / m3; natural river sand is medium sand, the fineness modulus is 2.3~3.0, and the average particle size is 0.5mm~0.3mm.
[0067] The preparation method of the heat-insulating hollow building block of this method is as follows:
[0068] Put the recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and stir, then pour in fly ash and silicate cement and mix and stir, then add natural river sand, gravel, straw fiber, aerogel, air entraining agent and water reducing agent in turn and mix and stir to obtain the block base material. The block base material is pressed into a hollow block by a vibration pressure molding machine. The foaming material is injected into the cavity of the hollow block, and then after standing and curing, the heat-insulating hollow block is obtained.
[0069] Comparative Example 3
[0070] The components of the thermal insulation hollow blocks in this example are as follows by weight:
[0071] 170 parts of fly ash, 270 parts of Portland cement, 430 parts of recycled coarse aggregate, 570 parts of gravel, 340 parts of recycled fine aggregate, 270 parts of natural river sand, 140 parts of hydrated sodium silicate, 70 parts of straw fiber, 30 parts of metallurgical slag, 170 parts of aerogel, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water.
[0072] The particle size of recycled coarse aggregate is 4.75mm~10.00mm, and the apparent density is 2050~2070kg / m 3 , water absorption rate is 9.6~9.7%; the particle size of recycled fine aggregate is <4.75mm, and the apparent density is 2310~2350kg / m3; natural river sand is medium sand, with a fineness modulus of 2.3~3.0 and an average particle size of 0.5mm~0.3mm.
[0073] The preparation method of the heat-insulating hollow building block of this method is as follows:
[0074] Put the recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and mix them, then pour in fly ash and silicate cement and mix them, then add natural river sand, gravel, straw fiber, air entraining agent, water reducing agent, water, aerogel in turn, and mix and mix to obtain the block base material. The block base material is pressed into a hollow block by a vibration pressure molding machine.
[0075] The foaming material is injected into the cavity of the hollow building block, and then the heat-insulating hollow building block is obtained after standing and curing.
[0076] Comparative Example 4
[0077] The components of the heat-insulating hollow building blocks in this embodiment are as follows by weight:
[0078] 170 parts of fly ash, 270 parts of Portland cement, 430 parts of recycled coarse aggregate, 570 parts of gravel, 340 parts of recycled fine aggregate, 270 parts of natural river sand, 80 parts of hydrated sodium silicate, 10 parts of straw fiber, 30 parts of metallurgical slag, 90 parts of aerogel, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water.
[0079] The particle size of recycled coarse aggregate is 4.75mm~10.00mm, the apparent density is 2050~2070kg / m3, and the water absorption rate is 9.6~9.7%; the particle size of recycled fine aggregate is <4.75mm, the apparent density is 2310~2350kg / m3; natural river sand is medium sand, the fineness modulus is 2.3~3.0, and the average particle size is 0.5mm~0.3mm.
[0080] The preparation method of the heat-insulating hollow building block of this method is as follows:
[0081] Put the recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and mix them, then pour in fly ash and silicate cement and mix them, then add natural river sand, gravel, straw fiber, air entraining agent, water reducing agent, water, aerogel in turn, and mix and mix to obtain the block base material. The block base material is pressed into a hollow block by a vibration pressure molding machine.
[0082] The foaming material is injected into the cavity of the hollow building block, and then the heat-insulating hollow building block is obtained after standing and curing.
[0083] The performance of the insulating hollow blocks obtained in Comparative Examples 1 to 4 and Examples 1 to 3 was tested. The compressive strength of the insulating hollow blocks was tested according to GB / T26538-2011 sintered insulating bricks and insulating blocks; Insulation performance, water absorption, and compressive strength of insulating hollow blocks.
[0084] Table 1 shows the performance of the self-insulating hollow blocks of the comparative example and the embodiment.
[0085]
[0086]
[0087] It can be seen from the test results of the embodiments and Table 1 that the present invention prepares a heat-insulating hollow block with high strength, good heat-insulating effect and low water absorption, and the method achieves this result by adding hydrated sodium silicate, straw fiber and aerogel. This is because hydrated sodium silicate can generate ceramic-like silicon dioxide crystals in long-term contact with air, which can effectively fill microcracks and pores, reduce the porosity of the block, and assist the bonding of cementitious materials and aggregates during the formation of the crystals. In addition, due to the permeability of hydrated sodium silicate, it can penetrate into the aggregate, improve the strength of the recycled aggregate, and reduce the number of pores, thereby achieving the effect of enhancing the strength of the block. Straw fiber can increase the tensile strength and impact resistance of concrete.
[0088] When straw fiber is added to building blocks, its fiber structure can form a network to increase the toughness and bearing capacity of concrete, thereby improving the overall mechanical properties of concrete, while controlling the shrinkage and cracking of concrete and having a good thermal insulation effect.
[0089] Example 1 is the best ratio, and its comprehensive performance of strength, thermal conductivity and water absorption is the highest. For details, please refer to Comparative Example 3 in which sodium silicate and straw fiber are added, and the compressive grade reaches MU5.0. At the same time, sodium silicate hydrate and straw fiber are irreplaceable, because sodium silicate hydrate can play a traction role on silica aerogel during stirring, so that the aerogel is more evenly attached to the vicinity of the straw fiber, so that the thermal insulation and waterproof performance of the aerogel is optimized.
[0090] In Example 2, the amount of aerogel added is relatively high, resulting in slightly lower strength and slightly better thermal insulation effect;
[0091] In Example 3, the amount of sodium silicate hydrate added is relatively small. Since sodium silicate hydrate plays a reinforcing role and a pulling effect on aerogel during the modification process, the small amount of sodium silicate hydrate added results in reduced strength of concrete, uneven dispersion of aerogel, slightly higher thermal conductivity, and slightly higher water absorption.
[0092] In Comparative Example 1, no sodium silicate hydrate, straw fiber and aerogel are added, and the strengthening effect of sodium silicate hydrate and straw fiber is lacking, resulting in lower strength of the building blocks. In the absence of thermal insulation and hydrophobic substances such as aerogel, the building blocks have poor thermal insulation effect and high water absorption.
[0093] In Comparative Example 2, only sodium silicate hydrate was added, and the strength of the blocks was obviously greatly improved.
[0094] In Comparative Example 3, the amount of aerogel added is too high, resulting in a higher thermal insulation effect of the building block than in Example 1. The strength of the building block is also reduced due to the high amount of aerogel added.
[0095] In comparative example 4, the amount of straw fiber added to the concrete is small, and the toughness and strength are reduced. Due to the traction of sodium silicate, the number of straw fibers is reduced, the dispersion degree of its aerogel is reduced, and the aerogel is unevenly dispersed, so that the thermal conductivity and water absorption are slightly higher.
[0096] Comparative Example 5
[0097] Under the conditions of Example 1, the addition amounts of hydrated sodium silicate, straw fiber and aerogel are controlled to be different, as follows:
[0098] Test 1: 120 parts of hydrated sodium silicate and 100 parts of aerogel;
[0099] Test 2: 60 parts of hydrated sodium silicate, 60 parts of straw fiber, and 100 parts of aerogel;
[0100] Test 3: 100 parts of hydrated sodium silicate, 40 parts of straw fiber, and 80 parts of aerogel;
[0101] Test 4: 100 parts of hydrated sodium silicate, 50 parts of straw fiber, and 70 parts of aerogel.
[0102] Table 2
[0103]
[0104] It can be seen that the present invention preferably uses 80 parts of hydrated sodium silicate, 50 parts of straw fiber, and 90 parts of aerogel, and the product has the best performance.
[0105] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing thermal insulation hollow blocks using recycled aggregate, characterized in that: include, Prepare the raw materials for the base material of the thermal insulation hollow block: according to the components by weight, 170 parts of fly ash, 270 parts of silicate cement, 430 parts of recycled coarse aggregate, 570 parts of gravel, 340 parts of recycled fine aggregate, 270 parts of natural river sand, 80 parts of hydrated sodium silicate, 50 parts of straw fiber, 30 parts of metallurgical slag, 90 parts of aerogel, 3 parts of air entraining agent, 6.2 parts of water reducer, and 120 parts of water; Preparation of block base material: Put recycled coarse aggregate, recycled fine aggregate and hydrated sodium silicate into a mixer and mix them evenly, then pour fly ash and silicate cement into the mixer and mix them, then add natural river sand, gravel, straw fiber, air entraining agent, water reducing agent, water and aerogel in sequence, mix and stir evenly to obtain the block base material; Preparation of hollow blocks: Pressing the block base material into hollow blocks by a vibration pressurizing molding machine; Preparation of thermal insulation hollow blocks: injecting unfoamed thermal insulation material stock solution into the cavity of the hollow block, accounting for 40% to 60% of the total volume of the cavity; after standing and curing, the foamed material completely fills the cavity of the block, thereby obtaining a thermal insulation hollow block; The fly ash, wherein the calcium oxide content is greater than 15%; The particle size of the recycled coarse aggregate is 4.75mm-10.0mm, and the apparent density is 2050-2070kg / m 3 , water absorption rate is 9.6~9.7%; The particle size of the recycled fine aggregate is less than 4.75 mm, and the apparent density is 2310-2350 kg / m 3 , water absorption rate is 9.5~9.6%; The natural river sand is medium sand, with a fineness modulus of 2.3 to 3.0 and an average particle size of 0.5 mm to 0.3 mm.
2. The method according to claim 1, characterized in that: The unfoamed thermal insulation material stock solution is prepared according to the following weight parts: 50-70 parts of phosphogypsum, 20-50 parts of fly ash, 5-10 parts of lime, 4-9 parts of hydrogen peroxide, 1-2 parts of foam stabilizer, 5-15 parts of silicon aerogel particles, and 20-60 parts of water.
3. The method according to claim 2, characterized in that: The foamed thermal insulation material is in liquid state before foaming, which is called unfoamed thermal insulation material stock solution. The preparation method thereof includes: The phosphogypsum is heated and fried at 170°C to obtain β-type hemihydrate phosphogypsum; Then, fly ash, lime and silicon aerogel particles are added thereto and mixed to obtain a mixture; Add hydrogen peroxide and foam stabilizer into warm water at 60-70°C, then pour water into the mixture and stir for 10-30 seconds to obtain the unfoamed thermal insulation material stock solution.
4. Preparation of thermal insulation hollow blocks using recycled aggregate obtained by the method described in any one of claims 1 to 3.