Preparation method and application of polyelectrolyte-based oil-absorbing gel asphalt modifier

Through the preparation of polyelectrolyte-based oil-absorbing gel asphalt modifiers, the problem of insufficient stability of traditional asphalt modifiers in high-temperature oxidation is solved, the performance and service life of asphalt are improved, and the asphalt flue gas is reduced. Pollution achieves more efficient modification effect.

CN116854850BActive Publication Date: 2024-11-12HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310715315.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-15
Publication Date
2024-11-12
Estimated Expiration
2043-06-15

AI Technical Summary

Technical Problem

Traditional asphalt modifiers have insufficient chemical and thermal stability during high-temperature oxidation, resulting in decomposition. Nanomaterial asphalt modifiers are costly and complex in process; the modification effect of oil-absorbing organic gels is low due to insufficient absorption capacity. .

Method used

The preparation method of polyelectrolyte-based oil-absorbing gel-based asphalt modifier is adopted, and the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT and Benzoyl oxide reacts under a nitrogen atmosphere to form a gel-based modifier with good chemical and thermal stability.

Benefits of technology

It significantly improves the viscoelastic performance, rut resistance and fatigue resistance of asphalt, reduces the release of volatile organic matter and micron-scale particles in asphalt flue gas, extends the service life of asphalt, and reduces air pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116854850B_ABST
    Figure CN116854850B_ABST
Patent Text Reader

Abstract

A preparation method and application of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier, which relates to a preparation method and application of an asphalt modifier. The purpose of the present invention is to solve the problem that the service life of asphalt pavement is greatly reduced due to the inability of traditional matrix asphalt road performance to meet actual traffic needs, and the current oil-absorbing organic gel asphalt modifier itself is insufficient, resulting in a low effect of improving the road performance of modified asphalt. Method: 1. Mix styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, acetone and benzoyl peroxide for reaction; 2. Heat the reaction under a nitrogen atmosphere; 3. Vacuum dry and freeze-dry to obtain a polyelectrolyte-based oil-absorbing gel-type asphalt modifier. A polyelectrolyte-based oil-absorbing gel-type asphalt modifier is used for modified asphalt. The present invention can obtain a polyelectrolyte-based oil-absorbing gel-type asphalt modifier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method and application of an asphalt modifier. Background Art

[0002] Asphalt pavement is widely used in highway pavement due to its short construction period, low noise, high friction and long durability. However, with the increase in traffic volume, vehicle load and ambient temperature, ordinary matrix asphalt with poor heat resistance and easy aging gradually cannot meet the requirements of pavement construction. Corresponding asphalt pavement diseases continue to occur, and the designed service life does not match the actual service life. Therefore, improving asphalt performance is one of the main research directions for improving asphalt pavement performance. At present, the main way to improve the performance of asphalt is to add asphalt modifiers, such as traditional asphalt modifiers represented by styrene-butadiene-styrene block copolymer (SBS), styrene-butadiene rubber (SBR), polyethylene glycol terephthalate (PET), etc.; environmentally friendly asphalt modifiers represented by waste rubber powder, recycled plastics, bio-asphalt, etc.; and nanomaterial asphalt modifiers represented by carbon nanotubes (CNTs), graphene (GNP), nano silica (Nano-SiO2), etc. Each modifier has a significant performance improvement effect on one or more road properties of asphalt. However, since the modification and aging of asphalt is a continuous high-temperature oxidation process, traditional and environmentally friendly asphalt modifiers generally have decomposition due to their own insufficient chemical / thermal stability. In addition, the cost of nanomaterial asphalt modifiers often needs to be used in combination with traditional or environmentally friendly asphalt modifiers, so the asphalt modification process is complicated and the cost is significantly increased. The development of a high-performance new asphalt modifier suitable for asphalt preparation and application environment is the focus of the current industry.

[0003] Oil-absorbing organogel is a porous organic polymer with a three-dimensional structure formed by cross-linking of one or more organic monomers through chemical reactions. Due to the existence of the porous structure, it can absorb a large amount of organic solvents and store them; it will also expand in volume due to the storage of a large amount of solvents. These functions are very similar to those of traditional asphalt modifiers, and in theory have similar modification effects on asphalt. In previous studies, it has been proven that it has the function of an asphalt modifier. In addition, since the volatile components of asphalt are partially absorbed by the oil-absorbing organogel, compared with unmodified asphalt, it will produce less asphalt fume during the application process, thus having an environmentally friendly function and helping to protect the health of construction workers. However, the modification effect of the oil-absorbing organogel is still somewhat different from that of the traditional asphalt modifier, which is due to the insufficient absorption capacity of the current oil-absorbing organogel for asphalt components. Therefore, based on the characteristics of the chemical composition of asphalt, how to scientifically design and regulate the molecular structure of the oil-absorbing organogel to enhance its swelling capacity in asphalt is the focus of current research on oil-absorbing organogel asphalt modifiers. Summary of the invention

[0004] The purpose of the present invention is to solve the problem that the service life of asphalt pavement is greatly reduced due to the inability of traditional matrix asphalt road performance to meet actual traffic needs, and the low effect of improving the road performance of modified asphalt due to the insufficient performance of current oil-absorbing organic gel asphalt modifiers themselves, and to provide a preparation method and application of a polyelectrolyte-based oil-absorbing gel asphalt modifier.

[0005] A method for preparing a polyelectrolyte-based oil-absorbing gel-type asphalt modifier is completed by the following steps:

[0006] 1. Add styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, acetone and benzoyl peroxide into a sealable container, and then stir at a certain speed to react at room temperature;

[0007] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is (1-5):(1-5):(0.03-0.15):(0.1-0.9):(0.06-0.3):(3-6);

[0008] The polyelectrolyte DTT described in step 1 is prepared according to the following steps:

[0009] ①. Preparation of anionic polyelectrolyte [DEMA-TD][Br]:

[0010] Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed and stirred for a period of time at the experimental temperature and in a nitrogen atmosphere to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, and the precipitate was collected and then vacuum dried to remove the solvent to obtain an anionic polyelectrolyte [DEMA-TD][Br], which was recorded as DTB;

[0011] The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone described in step ① is (1-2):1:(0.01-0.09):(3-6);

[0012] ②. Preparation of composite polyelectrolyte:

[0013] DTB, sodium tetraphenylborate and acetone were mixed and stirred for a period of time at the experimental temperature and nitrogen atmosphere to obtain a light yellow opaque liquid; a certain amount of deionized water was added dropwise to the light yellow opaque liquid at the experimental temperature and stirred for a certain period of time to obtain a white precipitate; the white precipitate was rinsed and finally vacuum dried to remove the residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], which was recorded as polyelectrolyte DTT;

[0014] The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step ② is 1:(1-2):(10-20):(30-60);

[0015] 2. Fill the container with nitrogen, seal the container, and then heat it under a nitrogen atmosphere for 5 h to 7 h to obtain a reaction product;

[0016] 3. The reaction product is first vacuum dried, then freeze dried, and finally crushed into powder to obtain a polyelectrolyte-based oil-absorbing gel-type asphalt modifier.

[0017] A polyelectrolyte-based oil-absorbing gel-type asphalt modifier is used for modifying asphalt.

[0018] The beneficial effects of the present invention are:

[0019] (1) The polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared by the present invention has good chemical and thermal stability;

[0020] (2) The viscoelastic properties, anti-rutting performance and anti-fatigue performance of the modified asphalt prepared by using the polyelectrolyte-based oil-absorbing gel asphalt modifier prepared by the present invention are greatly improved (compared with the base asphalt used in the control group, the phase angle is reduced by 7.33%~10.07%; the rutting factor is increased by 21.08%~84.55%; the theoretical fatigue life (complex modulus change rate = 0.5) is increased by 14.14%~142.07%); the polyelectrolyte-based oil-absorbing gel asphalt modifier prepared by the present invention can effectively improve the shortcomings of poor road performance and durability of the base asphalt;

[0021] (3) The polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared by the present invention requires a relatively low temperature when used for asphalt modification. The modified asphalt prepared by the polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared by the present invention can reduce the release of 41.91% of volatile organic matter and 29.0% of micron-sized particles in asphalt fume, which proves that the polyelectrolyte-based oil-absorbing gel-type asphalt modifier can solve the air pollution problem caused by asphalt fume generated during asphalt production and application to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is an infrared spectrum, in which 1 is styrene monomer, 2 is ethylene glycol dimethacrylate monomer,

[0023] 3 is octadecyl methacrylate monomer, 4 is polyelectrolyte DTT, and 5 is a polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1;

[0024] Figure 2 This is a thermogravimetric characterization spectrum of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1;

[0025] Figure 3 The graph of the phase angle of the base asphalt and the modified asphalt prepared in the application test 1 as a function of temperature is shown in FIG. 1 , which is the base asphalt prepared in the comparative example, and 2 , which is the modified asphalt prepared in the application test 1;

[0026] Figure 4 The figure is a curve diagram of the rutting factor of the base asphalt and the modified asphalt prepared in the application test 1 as a function of temperature, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 1;

[0027] Figure 5 The graph is a graph showing the change rate of the complex modulus of the base asphalt and the modified asphalt prepared in the application test 1 over time, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 1;

[0028] Figure 6The graph is a graph showing the phase angle of the base asphalt and the modified asphalt prepared in the application test 2 as a function of temperature, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 2;

[0029] Figure 7 The figure is a curve diagram of the rutting factor of the base asphalt and the modified asphalt prepared in the application test 2 as a function of temperature, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 2;

[0030] Figure 8 The graph is a graph showing the change rate of the complex modulus of the base asphalt and the modified asphalt prepared in the application test 2 over time, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 2;

[0031] Fig. 9 The graph is a graph showing the phase angle of the base asphalt and the modified asphalt prepared in the application test 3 as a function of temperature, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 3;

[0032] Fig.10 The figure is a curve diagram of the rutting factor of the base asphalt and the modified asphalt prepared in the application test 3 as a function of temperature, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 3;

[0033] Fig.11 The graph is a graph showing the change rate of the complex modulus of the base asphalt and the modified asphalt prepared in the application test 3 over time, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 3;

[0034] Fig.12 This is a comparison of the fluorescence microscope test results of the modified asphalt prepared in application test 1 under different aging conditions. In the figure, a is the original state (without aging treatment), and b is the long-term aging state;

[0035] Fig.13 This is a comparison chart of the gas chromatography-mass spectrometry test results of asphalt fumes released by base asphalt and modified asphalt prepared in application test 1 at 165°C for 1 hour, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in application test 1. DETAILED DESCRIPTION

[0036] Specific implementation method 1: In this implementation method, a method for preparing a polyelectrolyte-based oil-absorbing gel-type asphalt modifier is completed by the following steps:

[0037] 1. Add styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, acetone and benzoyl peroxide into a sealable container, and then stir at a certain speed to react at room temperature;

[0038] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is (1-5):(1-5):(0.03-0.15):(0.1-0.9):(0.06-0.3):(3-6);

[0039] The polyelectrolyte DTT described in step 1 is prepared according to the following steps:

[0040] ①. Preparation of anionic polyelectrolyte [DEMA-TD][Br]:

[0041] Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed and stirred for a period of time at the experimental temperature and in a nitrogen atmosphere to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, and the precipitate was collected and then vacuum dried to remove the solvent to obtain an anionic polyelectrolyte [DEMA-TD][Br], which was recorded as DTB;

[0042] The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone described in step ① is (1-2):1:(0.01-0.09):(3-6);

[0043] ②. Preparation of composite polyelectrolyte:

[0044] DTB, sodium tetraphenylborate and acetone were mixed and stirred for a period of time at the experimental temperature and nitrogen atmosphere to obtain a light yellow opaque liquid; a certain amount of deionized water was added dropwise to the light yellow opaque liquid at the experimental temperature and stirred for a certain period of time to obtain a white precipitate; the white precipitate was rinsed and finally vacuum dried to remove the residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], which was recorded as polyelectrolyte DTT;

[0045] The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step ② is 1:(1-2):(10-20):(30-60);

[0046] 2. Fill the container with nitrogen, seal the container, and then heat it under a nitrogen atmosphere for 5 h to 7 h to obtain a reaction product;

[0047] 3. The reaction product is first vacuum dried, then freeze dried, and finally crushed into powder to obtain a polyelectrolyte-based oil-absorbing gel-type asphalt modifier.

[0048] Specific embodiment 2: This embodiment differs from specific embodiment 1 in that the mass ratio of styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is 1:5:0.03:0.1:0.06:3. The other steps are the same as those in specific embodiment 1.

[0049] Specific embodiment 3: This embodiment differs from specific embodiment 1 or 2 in that the mass ratio of styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone in step 1 is 3:3:0.09:0.5:0.18:4.5. The other steps are the same as those in specific embodiment 1 or 2.

[0050] Specific embodiment 4: This embodiment differs from specific embodiments 1 to 3 in that the mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone in step 1 is 5:1:0.15:0.9:0.3:6. The other steps are the same as those in specific embodiments 1 to 3.

[0051] Specific embodiment 5: This embodiment differs from specific embodiments 1 to 4 in that: the stirring reaction time in step 1 is 1 h to 3 h, the stirring speed is 100 r / min to 800 r / min, and the room temperature in step 1 is 20° C. to 30° C. The other steps are the same as those in specific embodiments 1 to 4.

[0052] Specific embodiment 6: This embodiment differs from specific embodiments 1 to 5 in that the heating temperature in step 2 is 70° C. to 80° C. The other steps are the same as those in specific embodiments 1 to 5.

[0053] Specific embodiment 7: This embodiment differs from specific embodiments 1 to 6 in that: the vacuum drying temperature in step 3 is 60°C to 90°C, and the vacuum drying time is 5h to 10h; the freeze drying temperature in step 3 is -10°C to -5°C, and the freeze drying time is 3h to 6h. The other steps are the same as those in specific embodiments 1 to 6.

[0054] Specific implementation method 8: In this implementation method, a polyelectrolyte-based oil-absorbing gel-type asphalt modifier is used to modify asphalt.

[0055] Specific embodiment 9: This embodiment differs from specific embodiments 1 to 8 in that: a polyelectrolyte-based oil-absorbing gel-type asphalt modifier is used to modify asphalt in accordance with the following steps:

[0056] The dried base asphalt is mixed with a polyelectrolyte-based oil-absorbing gel-type asphalt modifier, and then sheared by a high-speed shearing machine at 130°C to 160°C to obtain a modified asphalt;

[0057] The mass ratio of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier to a dry base asphalt is (1-5):(50-100). The other steps are the same as those of the first to eighth embodiments.

[0058] Specific embodiment 10: This embodiment differs from specific embodiments 1 to 9 in that the shearing speed is 3000 r / min to 6000 r / min, and the shearing time is 20 min to 60 min. The other steps are the same as those of specific embodiments 1 to 9.

[0059] The following examples are used to verify the beneficial effects of the present invention:

[0060] Example 1: A method for preparing a polyelectrolyte-based oil-absorbing gel-type asphalt modifier is completed by the following steps:

[0061] 1. Add styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone into a sealable container, and then stir at room temperature (20°C) and a stirring speed of 100 r / min for 3 hours;

[0062] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is 1:5:0.03:0.1:0.06:3;

[0063] 2. Filling the container with nitrogen, then sealing the container, and maintaining it under the conditions of nitrogen atmosphere and temperature of 70° C. for 7 hours to obtain a reaction product;

[0064] 3. The reaction product is first vacuum dried at 60°C for 10 hours, then freeze-dried at -85°C for 3 hours, and finally crushed into powder to obtain a polyelectrolyte-based oil-absorbing gel-type asphalt modifier.

[0065] Example 2: A method for preparing a polyelectrolyte-based oil-absorbing gel-type asphalt modifier is completed by the following steps:

[0066] 1. Add styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone into a sealable container, and stir at room temperature (25°C) and a stirring speed of 450 r / min for 2 hours;

[0067] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is 3:3:0.09:0.5:0.18:4.5;

[0068] 2. Filling the container with nitrogen, then sealing the container, and maintaining it under the conditions of nitrogen atmosphere and temperature of 75° C. for 6 hours to obtain a reaction product;

[0069] 3. The reaction product is first vacuum dried at 75°C for 7.5 hours, then freeze-dried at -45°C for 4.5 hours, and finally crushed into powder to obtain a polyelectrolyte-based oil-absorbing gel-type asphalt modifier.

[0070] Example 3: A method for preparing a polyelectrolyte-based oil-absorbing gel-type asphalt modifier is completed by the following steps:

[0071] 1. Add styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone into a sealable container and then heat at room temperature (30 o C) and stirring at a speed of 800 r / min for 1 h;

[0072] The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is 5:1:0.15:0.9:0.3:6;

[0073] 2. Filling the container with nitrogen, then sealing the container, and maintaining it under the conditions of nitrogen atmosphere and temperature of 80° C. for 5 hours to obtain a reaction product;

[0074] 3. The reaction product is first vacuum dried at 90°C for 5 hours, then freeze-dried at -5°C for 3 hours, and finally crushed into powder to obtain a polyelectrolyte-based oil-absorbing gel-type asphalt modifier.

[0075] The preparation methods of the polyelectrolyte DTT described in Examples 1, 2 and 3 are the same, and are all completed according to the following steps:

[0076] 1. Preparation of anionic polyelectrolyte [DEMA-TD] [Br]:

[0077] Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed, stirred at 35°C and nitrogen atmosphere for 36 hours at a stirring speed of 800 r / min to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, the precipitate was collected, and the precipitate was vacuum dried to remove the solvent to obtain anionic polyelectrolyte [DEMA-TD][Br], recorded as DTB;

[0078] The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone in step 1 is 1:1:0.01:3;

[0079] 2. Preparation of composite polyelectrolyte:

[0080] DTB, sodium tetraphenylborate and acetone were mixed, stirred at 15°C and nitrogen atmosphere for 6 hours at a stirring speed of 800 r / min to obtain a light yellow opaque liquid; a certain amount of deionized water was added dropwise to the light yellow opaque liquid at 15°C, and stirred for another 12 hours at a stirring speed of 800 r / min to obtain a white precipitate; the white precipitate was rinsed with deionized water for 5 times, and finally vacuum dried to remove residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], which was recorded as polyelectrolyte DTT;

[0081] The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step 2 is 1:1:10:30.

[0082] Application Test 1: A polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1 is used to modify asphalt, which is specifically completed in the following steps:

[0083] The dried base asphalt was mixed with a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 1, and then sheared by a high-speed shearing machine at 130° C. and a shearing speed of 3000 r / min for 20 min to obtain a modified asphalt;

[0084] The mass ratio of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1 to dry base asphalt is 1:100.

[0085] Application Test 2: A polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 2 is used to modify asphalt, which is specifically completed in the following steps:

[0086] The dried base asphalt was mixed with a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 2, and then sheared by a high-speed shearing machine at 145° C. and a shearing speed of 4500 r / min for 40 min to obtain a modified asphalt;

[0087] The mass ratio of a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 2 to dry base asphalt is 5:100.

[0088] Application Test 3: A polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 3 is used to modify asphalt, which is specifically completed in the following steps:

[0089] The dried base asphalt was mixed with a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 3, and then sheared by a high-speed shearing machine at 160° C. and a shearing speed of 6000 r / min for 60 min to obtain a modified asphalt;

[0090] The mass ratio of a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 3 to dry base asphalt is 5:50.

[0091] Comparative Example:

[0092] The dried base asphalt was sheared by a high-speed shearing machine at 130°C and a shearing speed of 4500 r / min for 60 minutes to obtain the base asphalt.

[0093] The base asphalt described in Example 1, Example 2, Example 3 and Comparative Example is: No. 90 asphalt.

[0094] Styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT and a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 1 were characterized by FT-IR, and the characterization spectra are shown in FIG. Figure 1 As shown;

[0095] Figure 1 is an infrared spectrum, in which 1 is styrene monomer, 2 is ethylene glycol dimethacrylate monomer,

[0096] 3 is octadecyl methacrylate monomer, 4 is polyelectrolyte DTT, and 5 is a polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1;

[0097] from Figure 1 It can be seen that styrene contains 1494.12 cm -1 、1602.19 cm -1 、1637.08 cm -1 , representing the vibration absorption peak of the benzene ring skeleton, and 1637.08 cm -1 It also represents the C=C stretching vibration absorption peak. The octadecyl methacrylate monomer and the ethylene glycol dimethacrylate monomer contain 1722.81 cm -1 and 1163.91 cm -1 , which represent the C=O stretching vibration absorption peak and the CO stretching vibration absorption peak, respectively. In addition, styrene, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer and polyelectrolyte DTT all contain 1637.08 cm -1By comparing the polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1, styrene, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer and polyelectrolyte DTT, it can be found that the test results of the polyelectrolyte-based oil-absorbing gel-type asphalt modifier do not appear at 1637.08 cm -1 The C=C stretching vibration absorption peak represented by the asphalt modifier disappears, indicating that a polyelectrolyte-based oil-absorbing gel-type asphalt modifier is produced by the addition reaction of styrene, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer and polyelectrolyte DTT through C=C and has a high degree of reaction, which can ensure that the material has high chemical stability. The different polyelectrolyte-based oil-absorbing gel-type asphalt modifiers obtained by Examples 1, 2 and 3 show the same absorption peak in the FT-IR test results, and the difference lies in the different intensities of the absorption peaks, so they are not shown here.

[0098] Figure 2 This is a thermogravimetric characterization spectrum of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1;

[0099] from Figure 2 It can be seen that the initial decomposition temperature of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1 is 325.77°C, which proves that it has good thermal stability. In addition, this temperature is much higher than the use temperature (160-210°C) during the production and preparation of asphalt and mixtures and the pavement paving process;

[0100] Through dynamic shear rheology test, the phase angle variation curves of the modified asphalt obtained in the application test 1 of the present invention and the base asphalt prepared in the comparative example with temperature are respectively detected ( Figure 3 , taking the test frequency of 10 Hz as an example), the curve of rutting factor changing with temperature ( Figure 4 , taking the test frequency of 10 Hz as an example) and the theoretical fatigue life ( Figure 5 As shown in Table 1, the test frequency is 10 Hz and the test temperature is 25 o C as an example).

[0101] Figure 3 The graph of the phase angle of the base asphalt and the modified asphalt prepared in the application test 1 as a function of temperature is shown in FIG. 1 , which is the base asphalt prepared in the comparative example, and 2 , which is the modified asphalt prepared in the application test 1;

[0102] Figure 4 The figure is a curve diagram of the rutting factor of the base asphalt and the modified asphalt prepared in the application test 1 as a function of temperature, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 1;

[0103] Figure 5 The graph is a graph showing the change rate of the complex modulus of the base asphalt and the modified asphalt prepared in the application test 1 over time, wherein 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 1;

[0104] The phase angle represents the proportion of viscoelastic properties of asphalt. The smaller the value, the greater the proportion of elastic properties. The rutting factor represents the anti-rutting performance of asphalt. The larger the value, the stronger the performance. The theoretical fatigue life times represent the anti-fatigue performance of asphalt. The larger the value, the stronger the performance. Figure 3-4 It can be seen that the phase angle of the modified asphalt after adding a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 1 gradually increases with the increase of temperature compared with the base asphalt, and the value of the modified asphalt prepared in Experiment 1 is always smaller than that of the base asphalt within the test range, indicating that the elastic properties of the modified asphalt prepared in Experiment 1 are improved; the rutting factors decrease with the increase of temperature, and are greater than those of the base asphalt within the test range, indicating that the anti-rutting ability of the modified asphalt added with a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 1 is significantly enhanced; Figure 5 As can be seen from Table 1, the number of theoretical fatigue life of the modified asphalt prepared by adding application test 1 is significantly increased compared with the base asphalt, which proves that the anti-fatigue performance of the modified asphalt prepared by application test 1 is improved. In summary, it is proved that the viscoelastic properties, anti-rutting ability and anti-fatigue ability of the modified asphalt prepared by application test 1 are significantly improved.

[0105] Table 1

[0106]

[0107] Through dynamic shear rheology test, the phase angle variation curves of the modified asphalt obtained in the application test 2 of the present invention and the base asphalt prepared in the comparative example with temperature are respectively detected ( Figure 6 , taking the test frequency of 10 Hz as an example), the curve of rutting factor changing with temperature ( Figure 7 , taking the test frequency of 10 Hz as an example) and the theoretical fatigue life ( Figure 8 As shown in Table 2, the test frequency is 10 Hz and the test temperature is 25 o C as an example).

[0108] The phase angle represents the proportion of viscoelastic properties of asphalt. The smaller the value, the greater the proportion of elastic properties. The rutting factor represents the anti-rutting performance of asphalt. The larger the value, the stronger the performance. The theoretical fatigue life times represent the anti-fatigue performance of asphalt. The larger the value, the stronger the performance. Figure 6-8It can be seen that the phase angle of the modified asphalt after adding a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 2 gradually increases with the increase of temperature compared with the base asphalt, and the value of the modified asphalt prepared in Experiment 2 is always smaller than that of the base asphalt within the test range, indicating that the elastic properties of the modified asphalt prepared in Experiment 2 are improved; the rutting factors decrease with the increase of temperature, and are greater than those of the base asphalt within the test range, indicating that the anti-rutting ability of the modified asphalt added with a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 2 is significantly enhanced; Figure 8 As can be seen from Table 2, the number of theoretical fatigue life of the modified asphalt prepared by adding application test 2 is significantly increased compared with the base asphalt, which proves that the anti-fatigue performance of the modified asphalt prepared by application test 2 is improved. In summary, it is proved that the viscoelastic properties, anti-rutting ability and anti-fatigue ability of the modified asphalt prepared by application test 2 are significantly improved.

[0109] Table 2

[0110]

[0111] Through dynamic shear rheology test, the phase angle variation curves of the modified asphalt obtained in the application test 3 of the present invention and the base asphalt prepared in the comparative example with temperature are respectively detected ( Fig. 9 , taking the test frequency of 10 Hz as an example), the curve of rutting factor changing with temperature ( Fig.10 , taking the test frequency of 10 Hz as an example) and the theoretical fatigue life ( Fig.11 As shown in Table 2, the test frequency is 10 Hz and the test temperature is 25 o C as an example).

[0112] The phase angle represents the proportion of viscoelastic properties of asphalt. The smaller the value, the greater the proportion of elastic properties. The rutting factor represents the anti-rutting performance of asphalt. The larger the value, the stronger the performance. The theoretical fatigue life times represent the anti-fatigue performance of asphalt. The larger the value, the stronger the performance. Figure 9-10 It can be seen that the phase angle of the modified asphalt after adding a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 3 gradually increases with the increase of temperature compared with the base asphalt, and the value of the modified asphalt prepared in Experiment 3 is always smaller than that of the base asphalt within the test range, indicating that the elastic properties of the modified asphalt prepared in Experiment 3 are improved; the rutting factors decrease with the increase of temperature, and are greater than those of the base asphalt within the test range, indicating that the anti-rutting ability of the modified asphalt added with a polyelectrolyte-based oil-absorbing gel asphalt modifier prepared in Example 3 is significantly enhanced; Fig.11As can be seen from Table 3, the number of theoretical fatigue life of the modified asphalt prepared by adding application test 3 is significantly increased compared with the base asphalt, which proves that the anti-fatigue performance of the modified asphalt prepared by application test 3 is improved. In summary, it is proved that the viscoelastic properties, anti-rutting ability and anti-fatigue ability of the modified asphalt prepared by application test 2 are significantly improved.

[0113] Table 3

[0114]

[0115] Fig.12 This is a comparison of the fluorescence microscope test results of the modified asphalt prepared in application test 1 under different aging conditions. In the figure, a is the original state (without aging treatment), and b is the long-term aging state;

[0116] from Fig.12 (a) The original state test results of the modified asphalt prepared in application test 1 show that the polyelectrolyte-based oil-absorbing gel-type asphalt modifier in the modified asphalt prepared in application test 1 is dark green in block form and is evenly dispersed in the asphalt. Fig.12 (b) The long-term aging state of the modified asphalt prepared in application test 1 shows that the modified asphalt prepared in application test 1 is still stable in the asphalt after high temperature and high pressure treatment, and its volume is significantly increased. The above test results show that the modified asphalt prepared in application test 1 can still ensure that it will not decompose after short-term and long-term aging, and has sufficient thermal stability. The modified asphalt prepared by application tests 1, 2 and 3 showed the same morphological changes in the fluorescence microscope (FM) test results. The difference lies in the different densities caused by the different addition amounts of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier, so it is not shown here.

[0117] Test of the emission of volatile organic compounds from asphalt smoke at a constant temperature using the modified asphalt prepared in Application Test 1:

[0118] Studies have shown that asphalt will produce a large amount of smoke under high temperature conditions, which mainly includes volatile organic compounds and micron-sized particles. Fig.13 The gas chromatography-mass spectrometry test results of the asphalt smoke released by the base asphalt and the modified asphalt prepared in the application test 1 at 165°C for 1 hour are compared. In the figure, 1 is the base asphalt prepared in the comparative example, and 2 is the modified asphalt prepared in the application test 1. Table 4 shows the statistical results of the abundance of volatile organic compounds in the smoke of the base asphalt and the modified asphalt prepared in the application test 1, as well as the mass of micron-sized particles obtained by filtration.

[0119] Table 4

[0120]

[0121] Depend on Fig.13 As can be seen from Table 4, the abundance of volatile organic compounds and the mass of micron-sized particles in the asphalt fume generated by the modified asphalt prepared in Application Test 1 are reduced by 41.91% and 29.0% respectively compared with the base asphalt. This proves that under the same test time and temperature, the mass of asphalt fume generated by the modified asphalt prepared in Application Test 1 is significantly less than that of the base asphalt, that is, the addition of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier prepared in Example 1 can effectively inhibit the generation of asphalt fume.

[0122] The modified asphalt prepared by applying tests 1, 2 and 3 showed similar effects in reducing asphalt smoke in the asphalt smoke quality test results. The difference lies in the amount of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier added. The larger the amount added, the less asphalt smoke quality results, so it is not shown here.

Claims

1. Application of a polyelectrolyte-based oil-absorbing gel asphalt modifier, Features A polyelectrolyte-based oil-absorbing gel-type asphalt modifier is used to modify asphalt, which is specifically completed in the following steps: The dried base asphalt is mixed with a polyelectrolyte-based oil-absorbing gel-type asphalt modifier, and then sheared by a high-speed shearing machine at 130°C to 160°C to obtain a modified asphalt; The mass ratio of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier to a dry base asphalt is (1-5):(50-100); The preparation method of the polyelectrolyte-based oil-absorbing gel asphalt modifier is completed by the following steps:

1. Add styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, acetone and benzoyl peroxide into a sealable container, and then stir at a certain speed to react at room temperature; The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is (1-5):(1-5):(0.03-0.15):(0.1-0.9):(0.06-0.3):(3-6); The polyelectrolyte DTT described in step 1 is prepared according to the following steps: ①. Preparation of anionic polyelectrolyte [DEMA-TD][Br]: Tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone were mixed and stirred for a period of time at the experimental temperature and in a nitrogen atmosphere to obtain a viscous liquid; excess anhydrous ether was added to the viscous liquid, and the precipitate was collected and then vacuum dried to remove the solvent to obtain an anionic polyelectrolyte [DEMA-TD][Br], which was recorded as DTB; The molar ratio of tetradecane bromide, dimethylaminoethyl methacrylate, 4-methoxyphenol and acetone described in step ① is (1-2):1:(0.01-0.09):(3-6); ②. Preparation of composite polyelectrolyte: DTB, sodium tetraphenylborate and acetone were mixed and stirred for a period of time at the experimental temperature and nitrogen atmosphere to obtain a light yellow opaque liquid; a certain amount of deionized water was added dropwise to the light yellow opaque liquid at the experimental temperature and stirred for a certain period of time to obtain a white precipitate; the white precipitate was rinsed and finally vacuum dried to remove the residual solvent and water to obtain a hydrophobic composite polyelectrolyte [DEMA-TD][TPB], which was recorded as polyelectrolyte DTT; The molar ratio of DTB, sodium tetraphenylborate, acetone and deionized water in step ② is 1:(1-2):(10-20):(30-60); 2. Fill the container with nitrogen, seal the container, and then heat it under a nitrogen atmosphere for 5 h to 7 h to obtain a reaction product; 3. The reaction product is first vacuum dried, then freeze dried, and finally crushed into powder to obtain a polyelectrolyte-based oil-absorbing gel-type asphalt modifier.

2. Application of a polyelectrolyte-based oil-absorbing gel asphalt modifier according to claim 1, Features The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is 1:5:0.03:0.1:0.06:

3.

3. Use of a polyelectrolyte-based oil-absorbing gel asphalt modifier according to claim 1, Features The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is 3:3:0.09:0.5:0.18:4.

5.

4. Use of a polyelectrolyte-based oil-absorbing gel asphalt modifier according to claim 1, Features The mass ratio of the styrene monomer, octadecyl methacrylate monomer, ethylene glycol dimethacrylate monomer, polyelectrolyte DTT, benzoyl peroxide and acetone described in step 1 is 5:1:0.15:0.9:0.3:

6.

5. Use of a polyelectrolyte-based oil-absorbing gel asphalt modifier according to claim 1, Features The stirring reaction time in step 1 is 1 h to 3 h, and the stirring speed is 100 r / min to 800 r / min; the room temperature in step 1 is 20° C. to 30° C.

6. Use of a polyelectrolyte-based oil-absorbing gel asphalt modifier according to claim 1, Features The heating temperature in step 2 is 70°C to 80°C.

7. Use of a polyelectrolyte-based oil-absorbing gel asphalt modifier according to claim 1, Features The temperature of vacuum drying described in step 3 is 60°C~90°C, and the time of vacuum drying is 5h~10h; the temperature of freeze drying described in step 3 is -85°C~-5°C, and the time of freeze drying is 3h~6h.

8. Use of a polyelectrolyte-based oil-absorbing gel-type asphalt modifier according to claim 1, Features The shearing speed is 3000r / min~6000r / min, and the shearing time is 20min~60min.