A pick and a method for preparing the pick by laser cladding

By laser cladding an iron-based transition coating and a nickel-based alloy tungsten carbide composite coating on the pick, combined with a gradient cooling process, the problems of pick wear and low bonding strength of the cladding layer are solved, and the hardness and resistance are significantly improved. Grindability, extending the service life of the pick.

CN116855937BActive Publication Date: 2024-10-15SHANDONG LAIYAN LASER TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310992881.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-08
Publication Date
2024-10-15
Estimated Expiration
2043-08-08

AI Technical Summary

Technical Problem

Picks quickly fail due to excessive wear during the coal mining process. In laser cladding technology, the bonding strength between the cladding layer and the base material is low, which can easily cause stress and cause coating cracking, reducing the strengthening effect.

Method used

Using a two-layer laser cladding method, an iron-based transition coating is first formed on the surface of the pick base material, and then a nickel-based alloy and tungsten carbide composite coating is formed on the surface, combined with a gradient cooling process to relieve residual stress and improve Bonding strength.

Benefits of technology

It significantly improves the hardness and wear resistance of the pick, ensures the high bonding strength between the cladding layer and the base material, avoids crack defects, and extends the service life of the pick.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116855937B_ABST
    Figure CN116855937B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of metal laser cladding, and in particular to a pick and a method for preparing the pick by laser cladding. The pick comprises a pick substrate, and a cladding layer is laser clad on the surface of the pick substrate, and the cladding layer comprises an iron-based transition coating and a nickel-based alloy and tungsten carbide composite coating; the iron-based transition coating is laser clad on the surface of the pick substrate, and the nickel-based alloy and tungsten carbide composite coating is laser clad on the surface of the iron-based transition coating. The preparation method comprises: S1, laser cladding stainless steel powder on the surface of the pick substrate to form an iron-based transition coating; S2, laser cladding a mixed powder of nickel-based alloy powder and tungsten carbide powder on the surface of the iron-based transition coating to form a nickel-based alloy and tungsten carbide composite coating; S3, gradient cooling of the pick substrate after laser cladding. The present invention adopts a two-layer coating method of laser cladding to strengthen the pick surface, and the obtained pick substrate and the cladding layer have excellent bonding strength, and the pick surface has high hardness and strong wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal laser cladding, and in particular to a pick and a method for preparing the pick by laser cladding. Background Art

[0002] The pick is an important component used in coal mining machines. Its function is to cut coal from the coal seam during the coal mining process. The pick is subjected to a large impact load during the cutting process and is the most susceptible to wear and damage. At present, the pick used for coal mining in the coal mining machinery industry is mostly made of heat-treated 42CrMo. Under continuous impact load conditions, the pick made of this material will quickly fail due to excessive wear and require frequent shutdowns for replacement. Therefore, the performance of the pick directly affects the working efficiency of the coal mining machine.

[0003] Laser cladding technology is a new surface modification technology that completely melts the cladding material and the metal substrate surface and quickly solidifies it. The cladding layer and the surface of the base material form a complete metallurgical bond. It is a "green and environmentally friendly processing process" with high processing efficiency, wide application range, low cladding layer dilution, and strong bonding. The laser cladding layer has a dense surface quality and a low dilution rate, and has been widely used in the coal machinery industry.

[0004] Laser cladding technology also has some problems that need to be solved urgently. For example, the large temperature difference during the sudden heating and cooling of the molten pool during the laser cladding process, and the large difference in thermal expansion coefficients between the cladding layer and the substrate can easily cause stress-induced cracking of the coating. In addition, the pick is subjected to a large impact load, and the pick head is always in a state of stress concentration, which makes it easier for the cladding layer with crack defects to fall off and fail, thereby greatly reducing the strengthening effect of the laser cladding coating on the pick. Summary of the invention

[0005] In order to solve the technical problems such as low bonding strength between the cladding layer and the substrate, the present invention provides a pick and a method for preparing the pick by laser cladding. The surface of the pick is strengthened by laser cladding of two layers of coating. The prepared pick substrate and the cladding layer have excellent bonding strength, and the surface hardness of the pick is high and the wear resistance is strong.

[0006] In the first aspect, the present invention provides a pick, including a pick substrate, a surface of the pick substrate is laser-clad with a cladding layer, the cladding layer includes an iron-based transition coating and a nickel-based alloy and tungsten carbide composite coating; the iron-based transition coating is laser-clad on the surface of the pick substrate, and the nickel-based alloy and tungsten carbide composite coating is laser-clad on the surface of the iron-based transition coating.

[0007] Furthermore, the bonding strength between the cladding layer and the pick substrate is 420-430 MPa, which is close to the tensile strength of 316L stainless steel.

[0008] In a second aspect, the present invention provides a method for preparing a pick by laser cladding, comprising the following steps:

[0009] S1. Laser cladding stainless steel powder on the surface of the pick base material to form an iron-based transition coating;

[0010] S2, laser cladding a mixed powder of nickel-based alloy powder and tungsten carbide powder on the surface of the iron-based transition coating to form a composite coating of nickel-based alloy and tungsten carbide;

[0011] S3. The base material of the pick after laser cladding is subjected to gradient cooling.

[0012] Furthermore, in step S1, the stainless steel powder is a spherical powder obtained by atomizing 316L stainless steel, the powder sphericity is ≥85%, and the powder particle size is 35-53 μm; the stainless steel powder includes the following chemical components in weight percentage: C 0.02%, Cr17.98%, Ni 10.75%, Mo 2.39%, Mn 1.20%, Nb 0.98%, W 0.12%, Si 0.03%, and the balance is Fe and unavoidable impurity elements.

[0013] Furthermore, in step S1, the process conditions of laser cladding are as follows: spot diameter of 3~5mm, line speed of 4000mm / min, power of 5000~6000w, powder feeding amount of 10~12g / min, overlap rate of 45%~50%, powder feeder gas flow rate of 8L / min, shielding gas flow rate of 12L / min, and cladding thickness of 0.3~0.4mm.

[0014] Furthermore, in step S2, the nickel-based alloy powder is a spherical powder obtained by atomizing a nickel-based alloy, with a sphericity of ≥85% and a powder particle size of 35-53 μm; the tungsten carbide powder is a spherical powder obtained by atomizing tungsten carbide, with a powder particle size of 53-150 μm.

[0015] Furthermore, in step S2, the nickel-based alloy powder includes the following chemical components in weight percentage: C 0.45%, Cr 5.8%, Fe 6.34%, B 2.0%, Si 0.25%, Mn 0.15%, V 0.10%, and the remainder is Ni and unavoidable impurity elements; the weight percentage of tungsten carbide powder in the mixed powder is 5%~50%.

[0016] Furthermore, in step S2, the process conditions of laser cladding are as follows: spot diameter of 3~5mm, line speed of 1000~1200mm / min, power of 4500~5500w, powder feeding amount of 20~24g / min, overlap rate of 45%~50%, powder feeder gas flow rate of 8L / min, shielding gas flow rate of 12L / min, and cladding thickness of 1.2~1.3mm.

[0017] Furthermore, in step S2, before the iron-based transition coating is laser clad on the surface, the pick base material on which the iron-based transition coating has been laser clad is preheated to a temperature of 300°C.

[0018] Furthermore, in step S3, the process conditions for gradient cooling are as follows: after the laser cladding of the pick substrate is completed, it is placed in a constant temperature box for insulation, the initial temperature of the constant temperature box is set to 300°C, and after insulation for 2 to 2.5 hours, the temperature is lowered to room temperature at a gradient of 50°C / h.

[0019] The beneficial effects of the present invention are as follows: the present invention laser-clads a layer of low-hardness iron-based transition coating on the surface of the pick substrate to reduce the residual stress concentration caused by the difference in thermal expansion coefficient between the nickel-based alloy and tungsten carbide composite coating and the substrate after heating, and the iron-based transition coating 316L stainless steel is a non-magnetic stainless steel material, and there is no spark phenomenon during grinding, which meets the safety requirements of mining machinery in use. At the same time, the present invention cooperates with the heat preservation and slow cooling process after laser cladding to slowly release the residual stress generated during the laser cladding process, avoid excessive concentration of residual stress and cracking of the cladding layer, and obtain a complete laser cladding strengthening coating without crack defects. The cladding layer has a high bonding strength with the pick substrate, and has the advantages of high hardness and strong wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0021] Figure 1 It is a diagram of the cladding strengthening area of ​​the pick substrate according to a specific embodiment of the present invention.

[0022] Figure 2 It is a gradient cooling curve diagram of the pick after cladding is completed in a specific embodiment of the present invention.

[0023] Figure 3 It is a microscopic layered structure diagram of the laser cladding position of the pick according to a specific embodiment of the present invention.

[0024] Figure 4 It is a physical appearance diagram of a pick obtained by a specific implementation method of the present invention.

[0025] Figure 5 It is a microstructure diagram of the warp cutting metallographic experiment at the cladding position of the pick according to a specific embodiment of the present invention.

[0026] Figure 6 This is a workpiece diagram after the pick is made according to a specific implementation method of the present invention and subjected to a shear test.

[0027] In the figure, 1-cutting substrate, 2-iron-based transition coating, 3-nickel-based alloy and tungsten carbide composite coating. DETAILED DESCRIPTION

[0028] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0029] The stainless steel powder used in the following embodiment is a spherical powder obtained by atomizing 316L stainless steel, the sphericity of the powder is ≥85%, and the powder particle size is 35-53 μm; the stainless steel powder includes the following chemical components in weight percentage: C 0.02%, Cr17.98%, Ni 10.75%, Mo 2.39%, Mn 1.20%, Nb 0.98%, W 0.12%, Si 0.03%, and the balance is Fe and unavoidable impurity elements.

[0030] The nickel-based alloy powder used in the following examples is a spherical powder obtained by gas atomization of a nickel-based alloy, with a sphericity of ≥85% and a powder particle size of 35-53 μm; the tungsten carbide powder is a spherical powder obtained by gas atomization of tungsten carbide, with a powder particle size of 53-150 μm.

[0031] The nickel-based alloy powder used in the following embodiment includes the following chemical components in weight percentage: C 0.45%, Cr5.8%, Fe 6.34%, B 2.0%, Si 0.25%, Mn 0.15%, V 0.10%, and the balance is Ni and unavoidable impurity elements; the weight percentage of tungsten carbide powder in the mixed powder is 5%~50%, and the nickel-based alloy powder and tungsten carbide powder are mixed using a powder mixing device. Before mixing, the inner wall of the equipment filling bin is cleaned with industrial alcohol to avoid mixing in excess impurities. When mixing powder, the equipment speed is set to 10r / min, and the mixing time is 10h. After the powder mixing is completed, a portion of the powder is randomly picked up with paper tape and placed under a microscope. It is observed that the tungsten carbide powder has a good distribution uniformity, and is placed in an oven for drying to remove moisture to meet the use requirements.

[0032] The material of the base material of the pick in the following embodiments is 42CrMo steel.

[0033] Example 1

[0034] A method for preparing a pick by laser cladding comprises the following steps:

[0035] (1) Determine the processing position of the pick base material, machine the cutter head of the pick base material, and use a lathe to remove the surface oxide scale of the pick base material cladding strengthening area. The removal amount is 0.1mm. The pick base material cladding strengthening area is as follows: Figure 1 As shown in the dotted box, the mixed powders of stainless steel powder, nickel-based alloy powder and tungsten carbide powder are placed in powder feeders respectively. The powder feeder uses pneumatic powder feeding, inert gas argon is used as powder feeding gas, and the weight percentage of tungsten carbide powder in the mixed powder is 20%.

[0036] (2) Stainless steel powder was laser clad on the surface of the pick substrate to form an iron-based transition coating. The process conditions of laser cladding were as follows: spot diameter of 4 mm, line speed of 4000 mm / min, power of 5500 w, powder feeding amount of 11 g / min, overlap rate of 45%~50%, powder feeder gas flow rate of 8 L / min, shielding gas flow rate of 12 L / min, and cladding thickness of 0.3~0.4 mm.

[0037] (3) A mixed powder of nickel-based alloy powder and tungsten carbide powder was laser clad on the surface of the iron-based transition coating to form a nickel-based alloy and tungsten carbide composite coating. The process conditions of laser cladding were as follows: spot diameter of 4 mm, line speed of 1100 mm / min, power of 5000 w, powder feeding amount of 22 g / min, overlap rate of 45%~50%, powder feeder gas flow rate of 8 L / min, shielding gas flow rate of 12 L / min, and cladding thickness of 1.2~1.3 mm.

[0038] (4) After the cladding is completed, the pick is placed in a constant temperature box for insulation. The initial temperature of the constant temperature box is set to 300°C. After 2.3 hours of insulation, the temperature is cooled at a temperature gradient of 50°C / h. The cooling curve is shown in the figure. Figure 2 As shown, remove the cutting teeth after cooling to room temperature.

[0039] Figure 3 The microscopic layered structure of the laser cladding position of the pick obtained in Example 1 is shown. It can be seen that a cladding layer is laser-clad on the surface of the pick substrate 1, and the cladding layer includes an iron-based transition coating 2 and a nickel-based alloy and tungsten carbide composite coating 1; the iron-based transition coating 2 is laser-clad on the surface of the pick substrate, and the nickel-based alloy and tungsten carbide composite coating 3 is laser-clad on the surface of the iron-based transition coating 2.

[0040] Figure 4 The actual appearance of the pick obtained in Example 1 is shown. After observation and PT flaw detection, it was found that there were no cracks on the surface of the pick.

[0041] Figure 5 The wire cutting metallographic experimental microstructure diagram of the pick cladding position obtained in Example 1 is shown. It can be seen that the spherical tungsten carbide in the cladding layer is relatively concentrated at one end close to the pick substrate, and the distribution is relatively reasonable.

[0042] Figure 6 The workpiece diagram of the pick obtained in Example 1 after the shear test is shown. The bonding strength value of the cladding layer and the pick substrate is 421.75 MPa, which is close to the tensile strength of 316L stainless steel. The bonding strength test result meets the use requirements.

[0043] Example 2

[0044] A method for preparing a pick by laser cladding comprises the following steps:

[0045] (1) Determine the processing position of the pick substrate, machine the cutter head of the pick substrate, remove the surface oxide scale of the pick cladding strengthening area with a lathe, and remove 0.1 mm. Place the mixed powders of stainless steel powder, nickel-based alloy powder and tungsten carbide powder in the powder feeder, which uses pneumatic powder feeding. The inert gas argon is used as the powder feeding gas. The weight percentage of tungsten carbide powder in the mixed powder is 5%.

[0046] (2) Stainless steel powder was laser clad on the surface of the pick substrate to form an iron-based transition coating. The process conditions of laser cladding were as follows: spot diameter of 3 mm, line speed of 4000 mm / min, power of 5000 w, powder feeding amount of 10 g / min, overlap rate of 45%, powder feeder gas flow rate of 8 L / min, shielding gas flow rate of 12 L / min, and cladding thickness of 0.3-0.4 mm.

[0047] (3) A mixed powder of nickel-based alloy powder and tungsten carbide powder was laser clad on the surface of the iron-based transition coating to form a nickel-based alloy and tungsten carbide composite coating. The process conditions of laser cladding were as follows: spot diameter of 3 mm, line speed of 1000-1200 mm / min, power of 4500 w, powder feeding amount of 20 g / min, overlap rate of 45%-50%, powder feeder gas flow rate of 8 L / min, shielding gas flow rate of 12 L / min, and cladding thickness of 1.2-1.3 mm.

[0048] (4) After the cladding is completed, the pick is placed in a constant temperature box for insulation. The initial temperature of the constant temperature box is set to 300°C. After insulation for 2 hours, the temperature is lowered at a temperature gradient of 50°C / h. The pick is taken out after it drops to room temperature.

[0049] After testing, the bonding strength value of the pick cladding layer and the pick substrate obtained in Example 2 is 419.21 MPa, which is close to the tensile strength of 316L stainless steel. The bonding strength test result meets the use requirements.

[0050] Example 3

[0051] A method for preparing a pick by laser cladding comprises the following steps:

[0052] (1) Determine the processing position of the pick substrate, machine the cutter head of the pick substrate, use a lathe to remove the surface oxide scale of the pick cladding strengthening area, and remove 0.1 mm. Place the mixed powders of stainless steel powder, nickel-based alloy powder and tungsten carbide powder in the powder feeder. The powder feeder uses pneumatic powder feeding. The inert gas argon is used as the powder feeding gas. The weight percentage of tungsten carbide powder in the mixed powder is 50%.

[0053] (2) Stainless steel powder was laser clad on the surface of the pick substrate to form an iron-based transition coating. The process conditions of laser cladding were as follows: spot diameter of 5 mm, line speed of 4000 mm / min, power of 6000 w, powder feeding amount of 12 g / min, overlap rate of 45%~50%, powder feeder gas flow rate of 8 L / min, shielding gas flow rate of 12 L / min, and cladding thickness of 0.3~0.4 mm.

[0054] (3) A mixed powder of nickel-based alloy powder and tungsten carbide powder was laser clad on the surface of the iron-based transition coating to form a nickel-based alloy and tungsten carbide composite coating. The process conditions of laser cladding were as follows: spot diameter of 5 mm, line speed of 1200 mm / min, power of 5500 w, powder feeding amount of 24 g / min, overlap rate of 45%~50%, powder feeder gas flow rate of 8 L / min, shielding gas flow rate of 12 L / min, and cladding thickness of 1.2~1.3 mm.

[0055] (4) After the cladding is completed, the pick is placed in a constant temperature box for insulation. The initial temperature of the constant temperature box is set to 300°C. After insulation for 2.5 hours, the temperature is lowered at a temperature gradient of 50°C / h. The pick is taken out after it drops to room temperature.

[0056] After testing, the bonding strength value of the pick cladding layer and the pick substrate obtained in Example 3 is 429.96 MPa, which is close to the tensile strength of 316L stainless steel. The bonding strength test result meets the use requirements.

[0057] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.

Claims

1. A pick, comprising a pick base material, It is characterized in that The surface of the pick base material is laser clad with a cladding layer, which includes an iron-based transition coating and a nickel-based alloy and tungsten carbide composite coating; the iron-based transition coating is laser clad on the surface of the pick base material, and the nickel-based alloy and tungsten carbide composite coating is laser clad on the surface of the iron-based transition coating; the bonding strength value of the cladding layer and the pick base material is 420~430MPa; The method for preparing the pick by laser cladding comprises the following steps: S1. Laser cladding stainless steel powder on the surface of the pick base material to form an iron-based transition coating; S2, laser cladding a mixed powder of nickel-based alloy powder and tungsten carbide powder on the surface of the iron-based transition coating to form a composite coating of nickel-based alloy and tungsten carbide; S3, the base material of the pick after laser cladding is subjected to gradient cooling; In step S1, the stainless steel powder is a spherical powder obtained by atomizing 316L stainless steel, the powder sphericity is ≥85%, and the powder particle size is 35-53 μm; the stainless steel powder includes the following chemical components in weight percentage: C 0.02%, Cr 17.98%, Ni10.75%, Mo 2.39%, Mn 1.20%, Nb 0.98%, W 0.12%, Si 0.03%, and the balance is Fe and unavoidable impurity elements; In step S1, the process conditions of laser cladding are: spot diameter of 3-5 mm, linear speed of 4000 mm / min, power of 5000-6000 w, powder feeding amount of 10-12 g / min, overlap rate of 45%-50%, powder feeder gas flow rate of 8 L / min, shielding gas flow rate of 12 L / min, and cladding thickness of 0.3-0.4 mm; In step S2, the nickel-based alloy powder includes the following chemical components in weight percentage: C 0.45%, Cr 5.8%, Fe 6.34%, B 2.0%, Si 0.25%, Mn 0.15%, V 0.10%, and the balance is Ni and unavoidable impurity elements; the weight percentage of tungsten carbide powder in the mixed powder is 5% to 50%; In step S2, the process conditions of laser cladding are: spot diameter of 3-5 mm, linear speed of 1000-1200 mm / min, power of 4500-5500 w, powder feeding amount of 20-24 g / min, overlap rate of 45%-50%, powder feeder gas flow rate of 8 L / min, shielding gas flow rate of 12 L / min, and cladding thickness of 1.2-1.3 mm; In step S3, the process conditions of gradient cooling are as follows: after the laser cladding of the pick substrate is completed, it is placed in a constant temperature box for insulation, the initial temperature of the constant temperature box is set to 300°C, and after insulation for 2-2.5 hours, the temperature is lowered to room temperature at a gradient of 50°C / h.

2. The pick according to claim 1, It is characterized in that In step S2, the nickel-based alloy powder is a spherical powder obtained by gas atomization of the nickel-based alloy, with a sphericity of ≥85% and a powder particle size of 35-53 μm; the tungsten carbide powder is a spherical powder obtained by gas atomization of tungsten carbide, with a powder particle size of 53-150 μm.

3. The pick according to claim 1, It is characterized in that In step S2, before laser cladding the surface of the iron-based transition coating, the pick base material on which the iron-based transition coating has been laser clad is preheated to a temperature of 300°C.

Citation Information

Cited By

  • Method for welding mining cutting pick through high-entropy alloy laser cladding

    CN120055531A

  • A method for laser cladding welding of high-entropy alloy mining picks

    CN120055531B