A thermoplastic elastomer flame retardant material for fire hose and preparation method thereof

By adding fluorinated nanosilica powder to PVC/NBR thermoplastic elastomer material and granulation using dynamic vulcanization technology and twin screw extruder, the problem of poor flame retardant performance of the material is solved, and fire water belts and other Good application and cost reduction in the field.

CN116874945BActive Publication Date: 2024-11-22ZHONG YU HOSES TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310682200.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-09
Publication Date
2024-11-22
Estimated Expiration
2043-06-09

AI Technical Summary

Technical Problem

The existing PVC/NBR thermoplastic elastomer materials have deteriorated flame retardant performance after adding a large amount of plasticizer, and calcium carbonate powder does not have flame retardant effect, making it difficult to meet the flame retardant performance requirements in the field of fire safety.

Method used

By adding fluorinated nanosilica powder as flame retardant, combined with dynamic vulcanization technology and twin-screw extruder granulation process, a thermoplastic elastomer flame retardant material for fire water belts was prepared, using hydrogen fluoride and silicon carbon layers. Isolate air and heat during combustion to improve the flame retardant properties of the material.

Benefits of technology

In the case of small usage, the material not only ensures mechanical properties, but also significantly improves the flame retardant effect. It is suitable for fire hoses and other fields, and has good hydrophobicity and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004277031300000081
    Figure BDA0004277031300000081
  • Figure BDA0004277031300000091
    Figure BDA0004277031300000091
Patent Text Reader

Abstract

The invention relates to a thermoplastic elastomer flame retardant material for a fire hose and a preparation method thereof. The material comprises the following components in parts by weight: 50 parts of PVC resin, 20-25 parts of NBR powder, 25-35 parts of plasticizer, 0.1-1 parts of antioxidant, 1-6 parts of stabilizer, 0.1-0.5 parts of lubricant, 0.1-1 parts of vulcanizer and at least 2 parts of flame retardant; the flame retardant is fluorinated nano silicon dioxide powder; the mixture is mixed, melted, extruded and granulated; the fluorinated nano silicon dioxide powder is obtained by sequentially adding alkali solution and silicon-source fluorosilicone into an alcohol-water dispersion of nano silicon dioxide for reaction; and the PVC / NBR thermoplastic elastomer material can ensure its mechanical properties and have a good flame retardant effect when a small amount of the flame retardant is used by adding a specific flame retardant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a thermoplastic elastomer flame retardant material for a fire hose and a preparation method thereof. Background Art

[0002] PVC and NBR have the advantages of wide raw material sources, good blending effect, simple preparation process, low cost and flexible adjustment of formulation process according to performance requirements. They are widely used in construction materials, automotive parts, daily necessities, cables and other fields. Among them, dynamic vulcanization technology has attracted the attention of academia and industry. Through dynamic vulcanization technology, thermoplastic elastomers with both rubber elasticity and plastic thermoplasticity can be obtained, fully demonstrating the hybrid advantages of the two polymer materials.

[0003] In the prior art, the rubber hose material for fire hoses is mostly TPU material. Due to its high cost, the use of TPU is subject to certain restrictions. More and more manufacturers hope that there will be a material with low cost, simple processing technology and meeting the flame retardant performance requirements.

[0004] At present, PVC / NBR thermoplastic elastomer materials often use DOP as a plasticizer and calcium carbonate powder as a filler. Since the flame retardant properties of PVC / NBR thermoplastic elastomers will be greatly reduced after adding a large amount of plasticizers, and a large amount of smoke and toxic and harmful gases will be generated during the combustion process, and calcium carbonate powder filler does not have a flame retardant effect, it is often difficult to meet the flame retardant performance requirements in the fields of fire safety. Summary of the invention

[0005] In order to solve the technical problem that the flame retardant performance of PVC / NBR thermoplastic elastomer materials is poor, a thermoplastic elastomer flame retardant material for fire hose and a preparation method thereof are provided. By adding a specific flame retardant, the PVC / NBR thermoplastic elastomer material can ensure its mechanical properties and have a good flame retardant effect when the usage amount is small.

[0006] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:

[0007] A thermoplastic elastomer flame retardant material for a fire hose, comprising the following components in parts by weight:

[0008] 50 parts of PVC resin, 20-25 parts of NBR powder, 25-35 parts of plasticizer, 0.1-1 parts of antioxidant, 1-6 parts of stabilizer, 0.1-0.5 parts of lubricant, 0.1-1 parts of vulcanizing agent, at least 2 parts of flame retardant;

[0009] The flame retardant is fluorinated nano silicon dioxide powder.

[0010] Furthermore, the fluorinated nano-silicon dioxide powder is obtained by the following method, comprising the following steps:

[0011] (1) forming a dispersion of nano-silicon dioxide and an alcohol-water solvent;

[0012] (2) Under heating conditions, adding alkaline solution to the dispersion, then dropping a silicon source, adding fluorosilicone after the silicon source is added, and continuing the reaction. After the reaction is completed, filtering, washing, drying, and grinding to obtain fluorinated nano-silica powder.

[0013] Preferably, the alcohol-water solvent is a mixture of one or more of methanol, ethanol, isopropanol and water, the mass fraction of alcohol in the alcohol-water solvent is 50-95%, and the alcohol is anhydrous ethanol; the alkali solution is an ammonia solution with a mass concentration of 25-28%; the silicon source is tetraethyl orthosilicate; the fluorosilicone is one or more of 1H,1H,2H,2H-perfluorodecyltriethoxysilane, heptadecafluorodecyltripropoxysilane, 1H,1H,2H,2H-perfluorodecyltrimethyloxysilane, tridecafluorooctyltrimethoxysilane, (1H,1H,2H,2H-perfluorotetradecyl)tri(ethoxy)silane, and 1H,1H,2H,2H-perfluorododecyltriethoxysilane.

[0014] Preferably, the dispersion in step (1) is formed by mixing the nano-silica with the alcohol-water solvent in a mass volume ratio of 1 g:(30-50) mL and then subjecting the mixture to ultrasonic dispersion for 30-60 min.

[0015] Preferably, the heating temperature in step (2) is 55-65° C., and the reaction time is 20-30 h.

[0016] Preferably, the mass ratio of the nano-silica, the silicon source and the fluorosilicone is (15-20):1:0.1; and the volume ratio of the alkali solution to the silicon source is (5-10):1.

[0017] Furthermore, the thermoplastic elastomer flame retardant material comprises the following components in parts by weight:

[0018] 50 parts of PVC resin, 20 parts of NBR powder, 30 parts of plasticizer, 0.1-1 parts of antioxidant, 2 parts of stabilizer, 0.1 parts of lubricant, 0.1 parts of vulcanizer, and 2-10 parts of flame retardant.

[0019] Preferably, the plasticizer is a mixture of DOP and DOA, and the mass ratio of the DOP to the DOA is 5:1; the antioxidant is BHT; the stabilizer is 181 stabilizer; the lubricant is stearic acid or its salt; and the vulcanizing agent is DCP.

[0020] Another aspect of the present invention provides a method for preparing the thermoplastic elastomer flame retardant material for the fire hose, comprising the following steps:

[0021] (1) according to the formula, PVC resin, plasticizer, antioxidant, stabilizer, lubricant, vulcanizer and flame retardant are put into a high-speed mixer, stirring is started at 500-1000 rpm and the temperature is raised to 100-110° C., mixing is stopped when the material temperature reaches 100° C., the mixture is cooled to below 40° C., NBR powder is added, stirring and mixing is carried out at 100-200 rpm for 10-20 minutes, and a mixed material is obtained;

[0022] (2) The mixture is melt-blended and extruded into granules to obtain a thermoplastic elastomer flame-retardant material for a fire hose.

[0023] Furthermore, the melt blending and extrusion granulation are carried out in a twin-screw extruder, the rotation speed of the twin-screw extruder is 350-400rpm, and the temperature of the fuselage heating zone is: 120-140℃, 130-150℃, 140-160℃, 145-165℃, 150-170℃, 160-180℃, 160-180℃, 160-180℃.

[0024] Beneficial technical effects:

[0025] PVC and NBR have similar cohesive energy density and solubility parameters and are both polar polymers, so they can be miscible in any proportion during processing. The dynamic vulcanization processing method is used, and the twin-screw extruder mixes, melts, shears, and plasticizes the mixed powders, so that the NBR powder is highly vulcanized, cross-linked, and dispersed in the polyvinyl chloride during the processing. The micro-regions of the rubber and plastic phases are both separated and connected in a certain form. These characteristics give the material the advantages of both NBR elasticity and PVC thermoplasticity.

[0026] The present invention mixes the powders and granulates them by a twin-screw extruder, which is more conducive to realizing continuous production in the factory and reducing the overall production cost compared with processing by an internal mixer.

[0027] The present invention uses fluorinated nano silicon dioxide powder as a flame retardant. After being compounded with PVC / NBR, it decomposes during combustion to produce non-combustible gas hydrogen fluoride, which has a large specific gravity and forms a gas film on the surface of the material, covering the solid phase surface of the polymer material, thereby isolating air and heat. More importantly, hydrogen fluoride can inhibit the chain reaction of polymer material combustion and play a role in removing free radicals. At the same time, since silicon has extremely high migration energy, it will form a flame-retardant silicon-carbon layer on the surface of the material during combustion, which also blocks air and heat.

[0028] The fluorinated nano-silicon dioxide powder of the present invention has good compatibility with PVC / NBR thermoplastic elastomer materials, and the fluorinated nano-silicon dioxide powder has excellent hydrophobicity and can give the PVC / NBR thermoplastic elastomer materials good hydrophobicity, which is beneficial for the material to maintain good mechanical properties and flame retardant properties under humid or even water-immersed conditions, and provides a good foundation for application in the fields of fire hoses and the like. DETAILED DESCRIPTION

[0029] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.

[0031] The experimental methods in the following examples without specifying specific conditions are usually measured according to national standards; if there is no corresponding national standard, it is carried out according to the general international standards or the standard requirements proposed by relevant enterprises. Unless otherwise specified, all parts are by weight and all percentages are by weight.

[0032] Example 1

[0033] A thermoplastic elastomer flame retardant material for a fire hose, comprising the following components in parts by weight:

[0034] 50 parts of PVC resin, 20 parts of NBR powder, 25 parts of DOP, 5 parts of DOA, 0.5 parts of BHT, 2 parts of 181 stabilizer, 0.1 parts of stearic acid, 0.2 parts of DCP, 2 parts of fluorinated nano-silica powder;

[0035] The preparation method of fluorinated nano silicon dioxide powder is as follows:

[0036] (1) adding nano-silicon dioxide to an ethanol aqueous solution (with an anhydrous ethanol content of 80 wt%), and dispersing the solution by ultrasound for 30 min to form a dispersion; wherein the mass volume ratio of the nano-silicon dioxide to the ethanol aqueous solution is 1 g:40 mL;

[0037] (2) Under stirring conditions at 60° C., adding an ammonia solution with a mass concentration of 25% to the dispersion, then dropping tetraethyl orthosilicate, and after the dropping is complete, adding 1H,1H,2H,2H-perfluorodecyltrimethylsilane, continuing the reaction for 20 hours, and then filtering, washing, drying, and grinding to obtain fluorinated nano-silica powder; wherein the mass ratio of the nano-silica, the tetraethyl orthosilicate, and the 1H,1H,2H,2H-perfluorodecyltrimethylsilane is 18.9:1:0.1; and the volume ratio of the ammonia solution to the tetraethyl orthosilicate is 8:1.

[0038] The preparation method of the thermoplastic elastomer flame retardant material for the fire hose is as follows:

[0039] (1) According to the formula, PVC resin, DOP, DOA, BHT, 181 stabilizer, stearic acid, DCP, and fluorinated nano-silicon dioxide powder were put into a high-speed mixer, stirred at 800 rpm and heated to 100° C. When the material temperature reached 100° C., mixing was stopped, cooled to below 40° C., NBR powder was added, stirred and mixed at 100 rpm for 20 min, and a mixed material was obtained;

[0040] (2) A twin-screw extruder is used to melt-blend the mixed materials and extrude and granulate them to obtain a thermoplastic elastomer flame retardant material for a fire hose; the rotation speed of the twin-screw extruder is 350 rpm, and the temperatures of the heating zones of the extruder body are 130°C, 140°C, 150°C, 150°C, 160°C, 170°C, 170°C, and 180°C, respectively.

[0041] Example 2

[0042] A thermoplastic elastomer flame retardant material for a fire hose, comprising the following components in parts by weight:

[0043] 50 parts of PVC resin, 20 parts of NBR powder, 25 parts of DOP, 5 parts of DOA, 0.5 parts of BHT, 2 parts of 181 stabilizer, 0.1 parts of stearic acid, 0.2 parts of DCP, 2.5 parts of fluorinated nano-silica powder;

[0044] The preparation method of fluorinated nano silicon dioxide powder is as follows:

[0045] (1) adding nano-silicon dioxide to an ethanol aqueous solution (the anhydrous ethanol content is 70 wt%), and dispersing the solution by ultrasound for 60 min to form a dispersion; wherein the mass volume ratio of the nano-silicon dioxide to the ethanol aqueous solution is 1 g:40 mL;

[0046] (2) Under stirring conditions at 65° C., adding an ammonia solution with a mass concentration of 25% to the dispersion, then dropping tetraethyl orthosilicate, and after the dropping, adding 1H,1H,2H,2H-perfluorodecyltrimethylsilane, continuing the reaction for 20 hours, and then filtering, washing, drying, and grinding to obtain fluorinated nano-silica powder; wherein the mass ratio of the nano-silica, the tetraethyl orthosilicate, and the 1H,1H,2H,2H-perfluorodecyltrimethylsilane is 18.9:1:0.1; and the volume ratio of the ammonia solution to the tetraethyl orthosilicate is 8:1.

[0047] The preparation method of the thermoplastic elastomer flame retardant material for the fire hose is as follows:

[0048] (1) according to the formula, PVC resin, DOP, DOA, BHT, 181 stabilizer, stearic acid, DCP, fluorinated nano-silicon dioxide powder were put into a high-speed mixer, stirred at 1000 rpm and heated to 100° C., when the material temperature reached 100° C., mixing was stopped, cooled to below 40° C., NBR powder was added, stirred and mixed at 200 rpm for 10 min, and a mixed material was obtained;

[0049] (2) A twin-screw extruder is used to melt-blend the mixed materials and extrude and granulate them to obtain a thermoplastic elastomer flame retardant material for a fire hose; the rotation speed of the twin-screw extruder is 400 rpm, and the temperatures of the heating zones of the extruder body are 120°C, 130°C, 140°C, 145°C, 150°C, 160°C, 160°C, and 170°C, respectively.

[0050] Example 3

[0051] A thermoplastic elastomer flame retardant material for a fire hose, comprising the following components in parts by weight:

[0052] 50 parts of PVC resin, 20 parts of NBR powder, 25 parts of DOP, 5 parts of DOA, 0.5 parts of BHT, 2 parts of 181 stabilizer, 0.1 parts of stearic acid, 0.2 parts of DCP, 1.5 parts of fluorinated nano-silica powder;

[0053] The preparation method of fluorinated nano silicon dioxide powder is as follows:

[0054] (1) adding nano-silicon dioxide to an ethanol aqueous solution (with an anhydrous ethanol content of 90 wt%), and dispersing the solution by ultrasound for 40 min to form a dispersion; wherein the mass volume ratio of the nano-silicon dioxide to the ethanol aqueous solution is 1 g:40 mL;

[0055] (2) Under stirring conditions at 55° C., adding an ammonia solution with a mass concentration of 25% to the dispersion, then dropping tetraethyl orthosilicate, and after the dropping, adding 1H,1H,2H,2H-perfluorodecyltrimethylsilane, continuing the reaction for 30 hours, and then filtering, washing, drying, and grinding to obtain fluorinated nano-silica powder; wherein the mass ratio of the nano-silica, the tetraethyl orthosilicate, and the 1H,1H,2H,2H-perfluorodecyltrimethylsilane is 18.9:1:0.1; and the volume ratio of the ammonia solution to the tetraethyl orthosilicate is 8:1.

[0056] The preparation method of the thermoplastic elastomer flame retardant material for the fire hose is as follows:

[0057] (1) According to the formula, PVC resin, DOP, DOA, BHT, 181 stabilizer, stearic acid, DCP, and fluorinated nano-silicon dioxide powder were put into a high-speed mixer, stirred at 500 rpm and heated to 100° C. When the material temperature reached 100° C., mixing was stopped, cooled to below 40° C., NBR powder was added, stirred and mixed at 200 rpm for 10 min, and a mixed material was obtained;

[0058] (2) A twin-screw extruder is used to melt-blend the mixed materials and extrude and granulate them to obtain a thermoplastic elastomer flame retardant material for a fire hose; the rotation speed of the twin-screw extruder is 400 rpm, and the temperatures of the heating zones of the extruder body are 140°C, 150°C, 160°C, 165°C, 170°C, 180°C, 180°C, and 180°C, respectively.

[0059] Example 4

[0060] A thermoplastic elastomer flame retardant material for a fire hose, comprising the following components in parts by weight:

[0061] 50 parts of PVC resin, 20 parts of NBR powder, 28 parts of DOP, 5 parts of DOA, 0.5 parts of BHT, 2 parts of 181 stabilizer, 0.1 parts of stearic acid, 0.2 parts of DCP, 2 parts of fluorinated nano-silica powder;

[0062] The preparation method of fluorinated nano silicon dioxide powder is as follows:

[0063] (1) adding nano-silicon dioxide to an ethanol aqueous solution (with an anhydrous ethanol content of 95 wt%), and dispersing the solution by ultrasound for 30 min to form a dispersion; wherein the mass volume ratio of the nano-silicon dioxide to the ethanol aqueous solution is 1 g:40 mL;

[0064] (2) Under stirring conditions at 60° C., adding an ammonia solution with a mass concentration of 25% to the dispersion, then dripping tetraethyl orthosilicate, and then adding 1H,1H,2H,2H-perfluorodecyltrimethylsilane, and continuing the reaction for 30 hours, and then filtering, washing, drying, and grinding to obtain fluorinated nano-silica powder; wherein the mass ratio of the nano-silica, the tetraethyl orthosilicate, and the 1H,1H,2H,2H-perfluorodecyltrimethylsilane is 18.9:1:0.1; and the volume ratio of the ammonia solution to the tetraethyl orthosilicate is 8:1.

[0065] The preparation method of the thermoplastic elastomer flame retardant material for the fire hose is as follows:

[0066] (1) According to the formula, PVC resin, DOP, DOA, BHT, 181 stabilizer, stearic acid, DCP, and fluorinated nano-silicon dioxide powder were put into a high-speed mixer, stirred at 800 rpm and heated to 100° C. When the material temperature reached 100° C., mixing was stopped, cooled to below 40° C., NBR powder was added, stirred and mixed at 200 rpm for 10 min, and a mixed material was obtained;

[0067] (2) A twin-screw extruder is used to melt-blend the mixed materials and extrude and granulate them to obtain a thermoplastic elastomer flame retardant material for a fire hose; the rotation speed of the twin-screw extruder is 400 rpm, and the temperatures of the heating zones of the extruder body are 130°C, 140°C, 150°C, 150°C, 160°C, 170°C, 170°C, and 180°C, respectively.

[0068] Example 5

[0069] A thermoplastic elastomer flame retardant material for a fire hose, comprising the following components in parts by weight:

[0070] 50 parts of PVC resin, 20 parts of NBR powder, 30 parts of DOP, 5 parts of DOA, 0.5 parts of BHT, 2 parts of 181 stabilizer, 0.1 parts of stearic acid, 0.2 parts of DCP, 2 parts of fluorinated nano-silica powder;

[0071] The preparation method of fluorinated nano silicon dioxide powder is as follows:

[0072] (1) adding nano-silicon dioxide to an ethanol aqueous solution (with an anhydrous ethanol content of 80 wt%), and dispersing the solution by ultrasound for 30 min to form a dispersion; wherein the mass volume ratio of the nano-silicon dioxide to the ethanol aqueous solution is 1 g:40 mL;

[0073] (2) Under stirring conditions at 60° C., adding an ammonia solution with a mass concentration of 25% to the dispersion, then dripping tetraethyl orthosilicate, and then adding 1H,1H,2H,2H-perfluorodecyltrimethylsilane, and continuing the reaction for 30 hours, and then filtering, washing, drying, and grinding to obtain fluorinated nano-silica powder; wherein the mass ratio of the nano-silica, the tetraethyl orthosilicate, and the 1H,1H,2H,2H-perfluorodecyltrimethylsilane is 18.9:1:0.1; and the volume ratio of the ammonia solution to the tetraethyl orthosilicate is 8:1.

[0074] The preparation method of the thermoplastic elastomer flame retardant material for the fire hose is as follows:

[0075] (1) According to the formula, PVC resin, DOP, DOA, BHT, 181 stabilizer, stearic acid, DCP, and fluorinated nano-silicon dioxide powder were put into a high-speed mixer, stirred at 800 rpm and heated to 100° C. When the material temperature reached 100° C., mixing was stopped, cooled to below 40° C., NBR powder was added, stirred and mixed at 100 rpm for 20 min, and a mixed material was obtained;

[0076] (2) A twin-screw extruder is used to melt-blend the mixed materials and extrude and granulate them to obtain a thermoplastic elastomer flame retardant material for a fire hose; the rotation speed of the twin-screw extruder is 350 rpm, and the temperatures of the heating zones of the extruder body are 130°C, 140°C, 150°C, 150°C, 160°C, 170°C, 170°C, and 180°C, respectively.

[0077] Example 6

[0078] A thermoplastic elastomer flame retardant material for a fire hose, comprising the following components in parts by weight:

[0079] 50 parts of PVC resin, 23 parts of NBR powder, 28 parts of DOP, 5 parts of DOA, 0.5 parts of BHT, 2 parts of 181 stabilizer, 0.1 parts of stearic acid, 0.2 parts of DCP, 2 parts of fluorinated nano-silica powder;

[0080] The preparation method of fluorinated nano silicon dioxide powder is as follows:

[0081] (1) adding nano-silicon dioxide to an ethanol aqueous solution (with an anhydrous ethanol content of 95 wt%), and dispersing the solution by ultrasound for 30 min to form a dispersion; wherein the mass volume ratio of the nano-silicon dioxide to the ethanol aqueous solution is 1 g:40 mL;

[0082] (2) Under stirring conditions at 60° C., adding an ammonia solution with a mass concentration of 25% to the dispersion, then dropping tetraethyl orthosilicate, and after the dropping is complete, adding 1H,1H,2H,2H-perfluorodecyltrimethylsilane, continuing the reaction for 20 hours, and then filtering, washing, drying, and grinding to obtain fluorinated nano-silica powder; wherein the mass ratio of the nano-silica, the tetraethyl orthosilicate, and the 1H,1H,2H,2H-perfluorodecyltrimethylsilane is 18.9:1:0.1; and the volume ratio of the ammonia solution to the tetraethyl orthosilicate is 8:1.

[0083] The preparation method of the thermoplastic elastomer flame retardant material for the fire hose is as follows:

[0084] (1) According to the formula, PVC resin, DOP, DOA, BHT, 181 stabilizer, stearic acid, DCP, and fluorinated nano-silicon dioxide powder were put into a high-speed mixer, stirred at 800 rpm and heated to 100° C. When the material temperature reached 100° C., mixing was stopped, cooled to below 40° C., NBR powder was added, stirred and mixed at 150 rpm for 15 minutes, and a mixed material was obtained;

[0085] (2) A twin-screw extruder is used to melt-blend the mixed materials and extrude and granulate them to obtain a thermoplastic elastomer flame retardant material for a fire hose; the rotation speed of the twin-screw extruder is 400 rpm, and the temperatures of the heating zones of the extruder body are 130°C, 140°C, 150°C, 150°C, 160°C, 170°C, 170°C, and 180°C, respectively.

[0086] Comparative Example 1

[0087] The material preparation and materials used in this comparative example are the same as those in Example 1, except that: fluorinated nano-silica is not prepared, but fluorosilicone and nano-silica are directly dry-modified, and the modified nano-silica replaces the fluorinated nano-silica powder (flame retardant).

[0088] Comparative Example 2

[0089] The material preparation and materials used in this comparative example are the same as those in Example 1, except that: in this comparative example, 2 parts by weight of calcium carbonate is substituted for 2 parts by weight of fluorinated nano-silicon dioxide powder (flame retardant).

[0090] Comparative Example 3

[0091] The material preparation and materials used in this comparative example are the same as those in Example 1, except that: in this comparative example, 4 parts by weight of calcium carbonate replaces 2 parts by weight of fluorinated nano-silicon dioxide powder (flame retardant).

[0092] Comparative Example 4

[0093] The material preparation and materials used in this comparative example are the same as those in Example 1, except that: in this comparative example, 6 parts by weight of calcium carbonate are used to replace 2 parts by weight of fluorinated nano-silicon dioxide powder (flame retardant).

[0094] The proportions of the materials in the examples are shown in Table 1.

[0095] Table 1 Ratio of each material in the embodiment

[0096]

[0097] The materials of the examples were used to prepare standard samples, and the mechanical properties, flame retardant properties and density of the standard samples were tested according to national standards. The test results are shown in Table 2.

[0098] Table 2 Performance of materials in examples and comparative examples

[0099]

[0100] As shown in Table 2, the material of the present invention has good flame retardant properties after adding a small amount of fluorinated nano-silicon dioxide as a flame retardant (the amount of flame retardant added is 4% of the mass of PVC resin), the limiting oxygen index can reach more than 30%, and the material has certain hydrophobic properties.

[0101] The material ratios of Example 1 and Comparative Examples 1-4 are shown in Table 3.

[0102] Table 3 Material ratios of Example 1 and Comparative Examples 1-4

[0103] Element Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 PVC resin 50 50 50 50 50 NBR powder 20 20 20 20 20 DOP 25 25 25 25 25 DOA 5 5 5 5 5 BHT 0.5 0.5 0.5 0.5 0.5 181 Stabilizer 2 2 2 2 2 Stearic acid 0.1 0.1 0.1 0.1 0.1 DCP 0.2 0.2 0.2 0.2 0.2 Flame retardants 2 2 0 0 0 Calcium carbonate 0 0 2 4 6

[0104] Standard samples were prepared using the materials of Example 1 and Comparative Examples 1-4, and the mechanical properties, flame retardant properties and density of the standard samples were tested according to national standards. The test results are shown in Table 4.

[0105] Table 4 Material properties of Example 1 and Comparative Examples 1-4

[0106] Element Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 <![CDATA[Density / g·cm -3 > 1.203 1.233 1.177 1.162 1.186 Tensile strength / MPa 13.15 14.22 12.5 11.97 10.68 Elongation at break / % 350.26 288.55 335.71 314.04 312.00 Oxygen index / % 32.0 29.9 26.4 26.8 24.6 Vertical burning level V0 V0 V1 V1 V2 Water contact angle / ° 111.3 105.0 99.5 96.3 95.5

[0107] As can be seen from Table 2, in Comparative Example 1, fluorosilane and nano-silica are dry-modified and then compounded with PVC / NBR. The limiting oxygen index of the obtained material is less than 30%, and the water contact angle is smaller than that of Example 1, and the hydrophobicity is relatively poor; in Comparative Examples 2-4, calcium carbonate is added to replace fluorinated nano-silica, and the flame retardant effect is poor. Even if the amount of calcium carbonate is increased to 6 parts by weight, the material does not have flame retardancy, the limiting oxygen index is less than 27%, and the hydrophobicity is poor.

[0108] The present invention, after compounding the flame retardant fluorinated nano silicon dioxide powder with PVC / NBR, decomposes and produces incombustible gas hydrogen fluoride when the material burns, which has a large specific gravity and forms a gas film on the surface of the material, covering the solid phase surface of the polymer material, achieving the effect of isolating air and heat; more importantly, hydrogen fluoride can inhibit the chain reaction of the combustion of the polymer material and play a role in removing free radicals; at the same time, since the silicon element has extremely high migration energy, it will form a flame-retardant silicon-carbon layer on the surface of the material when burning, which also blocks air and heat. In addition, the fluorinated nano silicon dioxide powder has good compatibility with the PVC / NBR thermoplastic elastomer material, and the fluorinated nano silicon dioxide powder has excellent hydrophobicity, which can give the PVC / NBR thermoplastic elastomer material a good hydrophobic effect, which is conducive to the material maintaining good mechanical properties and flame retardant properties when it is wet or even immersed in water, and provides a good foundation for application in the fields of fire hoses.

[0109] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A thermoplastic elastomer flame retardant material for fire hose, characterized in that: It includes the following components by weight: 50 parts of PVC resin, 20-25 parts of NBR powder, 25-35 parts of plasticizer, 0.1-1 parts of antioxidant, 1-6 parts of stabilizer, 0.1-0.5 parts of lubricant, 0.1-1 parts of vulcanizing agent, at least 2 parts of flame retardant; The flame retardant is fluorinated nano silicon dioxide powder; The fluorinated nano-silicon dioxide powder is obtained by the following method, comprising the following steps: (1) forming a dispersion of nano-silicon dioxide and an alcohol-water solvent; (2) adding an alkali solution to the dispersion under heating conditions, then dropping a silicon source, adding fluorosilicone after the silicon source is added, and continuing the reaction. After the reaction is completed, filtering, washing, drying, and grinding to obtain fluorinated nano-silica powder; The alcohol-water solvent is a mixture of one or more of methanol, ethanol, isopropanol and water, wherein the mass fraction of alcohol in the alcohol-water solvent is 50-95%; the alkali solution is an ammonia solution with a mass concentration of 25-28%; the silicon source is tetraethyl orthosilicate; and the fluorosilicone is one or more of 1H,1H,2H,2H-perfluorodecyltriethoxysilane, heptadecafluorodecyltripropoxysilane, 1H,1H,2H,2H-perfluorodecyltrimethyloxysilane, tridecafluorooctyltrimethoxysilane, (1H,1H,2H,2H-perfluorotetradecyl)tri(ethoxy)silane, and 1H,1H,2H,2H-perfluorododecyltriethoxysilane.

2. The thermoplastic elastomer flame retardant material for fire hose according to claim 1, characterized in that: The dispersion in step (1) is formed by mixing the nano-silica with the alcohol-water solvent in a mass volume ratio of 1 g:(30-50) mL and then ultrasonically dispersing the mixture for 30-60 min.

3. The thermoplastic elastomer flame retardant material for fire hose according to claim 1, characterized in that: The heating temperature in step (2) is 55-65° C., and the reaction time is 20-30 h.

4. The thermoplastic elastomer flame retardant material for fire hose according to claim 1, characterized in that: The mass ratio of the nano-silica, the silicon source and the fluorosilicone is (15-20):1:0.1; the volume ratio of the alkali solution to the silicon source is (5-10):

1.

5. A thermoplastic elastomer flame retardant material for a fire hose according to any one of claims 1 to 4, characterized in that: The thermoplastic elastomer flame retardant material comprises the following components in parts by weight: 50 parts of PVC resin, 20 parts of NBR powder, 30 parts of plasticizer, 0.1-1 parts of antioxidant, 2 parts of stabilizer, 0.1 parts of lubricant, 0.1 parts of vulcanizer, and 2-10 parts of flame retardant.

6. The thermoplastic elastomer flame retardant material for fire hose according to claim 5, characterized in that: The plasticizer is a mixture of DOP and DOA, and the mass ratio of DOP to DOA is 5:1; the antioxidant is BHT; the stabilizer is 181 stabilizer; the lubricant is stearic acid or its salt; The vulcanizing agent is DCP.

7. The method for preparing the thermoplastic elastomer flame retardant material for fire hose according to any one of claims 1 to 6, characterized in that: The steps include: (1) according to the formula, PVC resin, plasticizer, antioxidant, stabilizer, lubricant, vulcanizer and flame retardant are put into a high-speed mixer, stirring is started at 500-1000 rpm and the temperature is raised to 100-110° C., mixing is stopped when the material temperature reaches 100° C., the mixture is cooled to below 40° C., NBR powder is added, stirring and mixing is carried out at 100-200 rpm for 10-20 minutes, and a mixed material is obtained; (2) The mixture is melt-blended and extruded into granules to obtain a thermoplastic elastomer flame-retardant material for fire hoses.

8. The method for preparing the thermoplastic elastomer flame retardant material for fire hose according to claim 7, characterized in that: The melt blending and extrusion granulation are carried out in a twin-screw extruder, the rotation speed of the twin-screw extruder is 350-400rpm, and the temperatures of the heating zones of the extruder body are 120-140°C, 130-150°C, 140-160°C, 145-165°C, 150-170°C, 160-180°C, 160-180°C, and 160-180°C.

Citation Information

Patent Citations

  • High-hydrophobicity and anti-adhering PVC-NBR (polyvinyl chloride-nitrile butadiene rubber) composite foam board and preparation method thereof

    CN106117916A

  • PVC / NBR cold-resistant oil-resistant flame retardant thermoplastic elastomer material for new energy automobile charging pile cable and preparation method thereof

    CN107880442A

  • Wear-resistant stain-resistant fluorenyl polyester master batch and high-transparency scratch-resistant antibacterial high-performance polycarbonate composite material

    CN111471286A

  • Method for preparing stable super-hydrophobic surface on complex modeling base material at super-fast speed

    CN114773921A

  • Manufacturing method for nonflammable organic-inorganic complex having hydro phobic property

    KR1020130102145A