A 750MPa grade steel plate for petroleum storage tanks and its production method
By reasonably controlling the chemical composition and heat treatment process of steel plates, the problem of difficult to take into account both the strength and welding performance of steel plates in the existing technology is solved, and the high strength, high toughness and good welding performance of steel plates for petroleum storage tanks is achieved, satisfying low welding cracks Sensitivity requirements while reducing production costs.
Patent Information
- Application Number
- CN202310909889.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-07-24
AI Technical Summary
It is difficult to develop a steel plate suitable for large-scale liquefied petroleum storage, which has excellent comprehensive performance, strength and toughness than conventional steel, and has similar welding performance or even better, and has a lower cost.
By reasonably controlling the chemical composition of the steel plate, including C, Si, Mn, Mo, Nb, Ti, V, Cu and Al content, using refined grain and precipitation strengthening technology, combined with staged rolling and tempering treatment, we ensure that Steel plates strike a balance between high strength and low weld crack sensitivity.
The high purity, high strength, high toughness and good welding performance of the steel plate for 750MPa grade petroleum storage tanks has been achieved, meeting the requirements of low welding crack sensitivity, and reducing production costs.
Smart Images

Figure CN116875904B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of steel preparation, and specifically relates to a 750MPa grade steel plate for oil storage tanks and a production method thereof, which is particularly suitable for containers for natural gas and crude oil transportation, oil refining and storage. Background Art
[0002] Strategic oil reserves are the main way to ensure oil security, which can maintain national economic stability and ensure economic security. As an important component of large storage tanks, the status of large storage tank steel cannot be ignored. Large storage tank steel must ensure that the base steel plate has high purity, high strength, high toughness and good welding performance, and meet the requirements of low welding crack sensitivity.
[0003] Invention patent CN202110836848.8 "A steel plate for petroleum storage tanks resistant to microbial corrosion and its manufacturing method" discloses a steel plate for petroleum storage tanks resistant to microbial corrosion and its manufacturing method, wherein the steel plate contains C: 0.03% to 0.10%, Si: 0.1% to 0.5%, Mn: 0.80% to 1.40%, P: less than 0.02%, S: less than 0.003%, Cu: 0.10% to 1.0%, Cr: 0.3% to 1%, Ni: 0.2% to 1.3%, Mo: 0.05% to 0.4%, Ti: 0.01% to 0.05%, V: 0.02% to 0.06%, RE: 0.05% to 0.1%, and the balance is Fe and unavoidable impurity elements. The addition of rare earth element RE in the steel plate makes the production cost of the steel plate high, and only the production of 20mm thickness steel plate is studied, which is not suitable for large-scale and full-series wide applications.
[0004] In view of the above situation, it is urgent to research and develop a large-scale liquefied petroleum storage steel plate with excellent comprehensive properties, whose strength and toughness are better than conventional steels, and whose welding performance is similar or even better, and whose cost is lower. Summary of the invention
[0005] In view of this, the object of the present invention is to provide a high-strength, high-toughness, low-crack-sensitivity steel plate for oil storage tanks with good comprehensive performance and a production method thereof.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] The invention provides a 750MPa grade steel plate for petroleum storage tanks. The chemical composition of the steel plate is as follows by weight percentage: C: 0.1%-0.16%, Si: 0.08%-0.10%, Mn: 0.6%-0.8%, P: ≤0.003%, S: ≤0.001%, Mo: 0.03%-0.045%, Nb: 0.035%-0.045%, Ti: 0.06%-0.075%, V: 0.01%-0.02%, Cu: 0.01%-0.06%, Als: 0.002%-0.03%, and the rest is Fe and unavoidable impurities.
[0008] The mechanism of action of the above chemical elements is as follows:
[0009] C: It often forms carbides with other alloy elements in steel to strengthen the steel plate, ensuring that the strength of the steel plate is maintained at a high level. However, a high C content is prone to segregation in the steel, resulting in a significant decrease in the toughness and plasticity of the steel plate, which is not conducive to ensuring the low welding crack sensitivity of the steel plate. In order to solve this problem, the present invention uses TiC to refine the grains. Therefore, under the premise of ensuring the strength of the steel plate, the C content is controlled at 0.1% to 0.16%.
[0010] Si: It has deoxidation and desulfurization effects in steel and can improve the strength of steel plates through solid solution strengthening. The procurement cost of Si is low, and adding an appropriate amount of Si in steel can ensure that the hardness and strength of ferrite in the steel are at a high level, and can improve the local corrosion resistance of the steel plate. However, if the Si content is high, the low-temperature impact absorption energy of the heat-affected zone of the steel plate is reduced. Therefore, the Si content in the designed steel should not be greater than 0.1%, so the Si content is limited to 0.08% to 0.10%.
[0011] Mn: The element is a commonly used desulfurizer in steel, and Mn is easy to form sulfide inclusions with S. Too high a content of Mn is easy to segregate to produce a hard paper phase, which reduces the welding performance of the steel plate and increases the sensitivity of welding cracks of the steel plate. Considering factors such as ensuring the strength, toughness and welding performance of the steel plate, the Mn content is set within the range of 0.6% to 0.8% during the composition design.
[0012] P and S are brittle elements in steel and are also elements that are extremely easy to segregate, so the lower their content, the better. They also have a great detrimental effect on the low-temperature toughness of steel. However, considering factors such as steelmaking operability, steelmaking cost, and meeting usage needs, the contents of P and S are controlled below 0.003% and 0.001%, respectively.
[0013] Mo: It is a weak solid solution strengthening element. It can refine the structure in steel, strengthen the steel plate and has a good effect on the impact toughness and brittle transition temperature. However, Mo is not conducive to the welding performance of the steel plate and has a high purchase cost. Therefore, in the present invention, the content of Mo is controlled to 0.03% to 0.045%.
[0014] Nb: As an important element of the patented steel plate, it has a significant effect on grain refinement and is easily combined with C. The NbC formed during hot rolling hinders the recovery and recrystallization of deformed austenite and promotes the transformation of deformed austenite structure rolled in the non-recrystallization zone into fine phase transformation products during phase transformation, which has a positive effect on the strength and toughness of the steel plate. Therefore, the present invention sets the Nb content to 0.035% to 0.045%.
[0015] Ti: As an important element of the patented steel plate, it is a strong carbonitride-forming element. It forms stable titanium carbide that is difficult to dissolve when heated, and can effectively inhibit the expansion of grain boundaries, reduce the size of austenite grains, increase the nucleation rate of ferrite, and reduce the probability of overheating of the steel plate during heat treatment. Secondly, Ti is also easy to form stable TiC with C, which serves the purpose of solidifying C, reducing the reaction with free C and H in steel, reducing the production of harmful substances such as methane, and reducing the decarburization, bulging and cracking tendency of the steel plate. TiC particles will precipitate in the austenite zone during heating, which will inhibit the recrystallization of austenite and prevent the growth of austenite grains. In addition, studies have shown that excessive Ti will cause abnormal growth of grains, which is not conducive to the low-temperature toughness and welding performance of the steel plate. Therefore, the Ti content is controlled within the range of 0.06% to 0.075%.
[0016] V: Similar to Ti, it combines with Nb and Ti elements and C in steel to play the role of precipitation strengthening, fine grain strengthening and precipitation strengthening, which is beneficial to ensure the strength and toughness of the steel plate and the welding performance, but excessive V will cause mixed crystal phenomenon in the steel plate. Therefore, the V content is set at 0.01% to 0.02%
[0017] Cu: improves the strength of steel through solid solution strengthening in steel, while ensuring the hardenability of the steel plate. However, excessive Cu is not conducive to the welding performance of the steel plate. Therefore, the present invention limits the Cu content to 0.01% to 0.06%.
[0018] Als: As a deoxidizing element in steel, it can effectively refine the grains in steel. The appropriate content is 0.002% to 0.03%.
[0019] Based on the above technical scheme, further, the thickness of the steel plate is 80-100 mm, the tensile strength is 750-850 MPa, the yield strength is 550-650 MPa, the elongation after fracture is 20%-25%, and the impact energy at -20°C is 200-250 J; the mechanical properties of the die-welded state are: tensile strength is 730-760 MPa, yield strength is 550-600 MPa, elongation after fracture is 25%-30%, and the impact energy at -20°C is 210-280 J.
[0020] Another aspect of the present invention provides a method for producing the above-mentioned 750MPa grade steel plate for petroleum storage tanks, which mainly comprises the following steps:
[0021] (1) Heating of continuous casting billet: The heating temperature of continuous casting billet is 1170-1250℃, and the soaking time is 2-4h. When the heating temperature is lower than 1170℃, the primary precipitates in the continuous casting billet are not completely dissolved, which affects the austenitization process and cannot effectively reach the rough rolling start and final rolling temperature; and it has an adverse effect on the grain size of the steel plate;
[0022] (2) Rolling of continuous casting billet: the starting rolling temperature of rough rolling is ≥1060℃, the single-pass reduction rate is 6-9%, and a large deformation amount is used for rapid rolling at this stage to ensure that the dynamic recrystallization process near the surface of the steel plate is complete; the starting rolling temperature of finishing rolling is ≥1000℃, the final rolling temperature is ≥820℃, and the single-pass reduction rate is 3-5%. At this stage, a small deformation amount is used for rapid rolling to ensure that no recrystallization occurs near the surface of the steel plate;
[0023] (3) Tempering treatment: The tempering temperature is controlled at 600-650°C and the furnace time is 2-4 hours.
[0024] Based on the above technical solution, further, in step (1), the heating temperature of the continuous casting billet is 1170-1220°C.
[0025] Based on the above technical solution, further, in step (2), the starting temperature of rough rolling is 1060-1170°C, and the final rolling temperature is 1040-1060°C; the starting temperature of fine rolling is 1000-1020°C, and the final rolling temperature is 820-840°C.
[0026] Based on the above technical solution, further, the tempering temperature in step (3) is controlled at 620-630°C.
[0027] Based on the above technical solution, further, the preparation of the continuous casting billet described in step (1) comprises the following steps:
[0028] Hot metal pretreatment - converter smelting - LF furnace refining - RH vacuum treatment - continuous casting;
[0029] Among them, during the continuous casting process, the casting temperature of molten steel is ≤1540℃ to refine the original cast structure. In order to reduce the probability of central segregation and looseness of the continuous casting billet, electromagnetic stirring or continuous casting billet light reduction process is adopted, and the billet light reduction rate is controlled at 5-7%.
[0030] Based on the above technical solution, further, the molten steel casting temperature is 1530-1540°C.
[0031] Based on the above technical solution, further, the molten iron pretreatment includes desulfurization and dephosphorization, and the sulfur mass fraction of the molten iron is reduced to below 0.003%, and the phosphorus mass fraction is reduced to below 0.001%.
[0032] Based on the above technical scheme, further, LF furnace refining is used to adjust the composition and deep desulfurization treatment is carried out, and RH vacuum treatment is used to further adjust the composition; among them, RH vacuum treatment is degassing (nitrogen, hydrogen, oxygen, etc.) to make the inclusions in the molten steel (sulfides, oxides, silicates, etc.) fully float, which is an effective way to fundamentally ensure the purity of the steel, and it is also an effective means of micro-alloying the steel.
[0033] Based on the above technical solution, further, slag blocking balls are added to block slag when steel is tapped from the converter.
[0034] Based on the above technical solution, further, the simulated welding heat treatment temperature of the steel plate is 570-590° C., and the net insulation time is 2-4 hours.
[0035] The beneficial effects of the present invention compared with the prior art are as follows:
[0036] 1. In order to ensure the high purity, high strength, high toughness and good welding performance of the steel plate and meet the requirements of low welding crack sensitivity, the present invention reasonably controls the C and Mn contents in the steel to ensure that the segregation degree of the steel plate is relatively light; at the same time, in order to ensure that the steel plate has good strength and toughness, alloy elements Nb, V, Ti, and Mo are added to the steel to refine the grains, and precipitation strengthening is used to ensure that the steel plate has good comprehensive properties after tempering and simulated post-weld heat treatment.
[0037] 2. The present invention adopts a heat treatment method of staged rolling and tempering to ensure that the finished steel plate has a uniform grain size and high strength throughout the thickness direction while having good welding performance and meeting the requirements of low welding crack sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention, the drawings related to the embodiments are briefly introduced below.
[0039] Figure 1 This is the metallographic structure of the steel plate prepared in the example. DETAILED DESCRIPTION
[0040] The present invention is described in detail below with reference to the embodiments, but the embodiments of the present invention are not limited thereto. Obviously, the embodiments described below are only partial embodiments of the present invention. For those skilled in the art, other similar embodiments obtained without creative labor all fall within the protection scope of the present invention.
[0041] Examples 1-6
[0042] This embodiment provides a 750MPa grade steel plate for oil storage tanks, the thickness, chemical composition and weight percentage of the steel plate are shown in Table 1;
[0043] Table 1 Chemical composition of the oil tank steel plates of Examples 1-6 (wt%)
[0044]
[0045] The production method comprises the following steps:
[0046] Hot metal pretreatment - converter smelting - LF furnace refining - RH vacuum treatment - continuous casting - heating - rolling - tempering - trimming - inspection and testing;
[0047] Among them, the hot metal pretreatment includes desulfurization and dephosphorization, and the sulfur mass fraction of the hot metal is reduced to below 0.003%, and the phosphorus mass fraction is reduced to below 0.001%;
[0048] LF furnace refining is used to adjust the composition and deep desulfurization treatment is carried out, and RH vacuum treatment is used to further adjust the composition;
[0049] The parameters of molten steel casting temperature and billet soft reduction rate during continuous casting are shown in Table 2;
[0050] The continuous casting billet heating temperature and soaking time during the heating process are shown in Table 2.
[0051] The rolling of the continuous casting billet adopts a two-stage controlled rolling process, wherein the starting rolling temperature, final rolling temperature, single-pass reduction rate of the rough rolling and the starting rolling temperature, final rolling temperature, single-pass reduction rate of the finishing rolling are shown in Table 2.
[0052] Table 2 Continuous casting and rolling process parameters of oil tank steel plates of Examples 1-6
[0053]
[0054] The rolled steel plate was tempered. The tempering temperature, heating rate and time in the furnace are shown in Table 3. The simulated post-weld heat treatment temperature and net holding time are shown in Table 3.
[0055] Table 3 Heat treatment process parameters of oil tank steel plates of Examples 1-6
[0056]
[0057] The mechanical properties of the prepared 750MPa grade steel plate for oil storage tanks are shown in Table 4, the mechanical properties of the die-welded state are shown in Table 5, and the grain size and non-metallic inclusion test results are shown in Table 6. The structure of the steel plate is tempered troostite, the structure in the steel is uniform, and the segregation is low.
[0058] Table 4 Mechanical properties of oil tank steel plates of Examples 1-6
[0059]
[0060] Table 5 Mechanical properties of the die-welded steel plates of the oil tanks of Examples 1-6
[0061]
[0062] Table 6 Grain size and non-metallic inclusion test results of oil tank steel plates of Examples 1-6
[0063]
[0064] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A 750MPa grade steel plate for petroleum storage tanks, characterized in that: The chemical composition of the steel plate is as follows by weight percentage: C: 0.1% to 0.16%, Si: 0.08% to 0.10%, Mn: 0.6% to 0.8%, P: ≤ 0.003%, S: ≤ 0.001%, Mo: 0.03% to 0.045%, Nb: 0.035% to 0.045%, Ti: 0.06% to 0.075%, V: 0.01% to 0.02%, Cu: 0.01% to 0.06%, Als: 0.002% to 0.03%, and the rest is Fe and unavoidable impurities; The steel plate has a thickness of 80 to 100 mm, a tensile strength of 750 to 850 MPa, a yield strength of 550 to 650 MPa, an elongation after fracture of 20% to 25%, and an impact energy of 200 to 250 J at -20°C; a simulated welding heat treatment temperature of 570 to 590°C, a net holding time of 2 to 4 hours, and mechanical properties of the mold-welded state: a tensile strength of 730 to 760 MPa, a yield strength of 550 to 600 MPa, an elongation after fracture of 25% to 30%, and an impact energy of 210 to 280 J at -20°C; The production method of the 750MPa grade steel plate for petroleum storage tanks comprises the following steps: (1) Heating of continuous casting billet: The heating temperature of continuous casting billet is 1170-1220℃, and the soaking time is 2-4h; (2) Rolling of continuous casting billet: the starting rolling temperature of rough rolling is 1060-1170°C, the final rolling temperature is 1040-1060°C, and the single-pass reduction rate is 6-9%; the starting rolling temperature of finishing rolling is 1000-1020°C, the final rolling temperature is 820-840°C, and the single-pass reduction rate is 3-5%; (3) Tempering treatment: The tempering temperature is controlled at 620-630°C and the furnace time is 2-4 hours.
2. The production method according to claim 1, characterized in that The preparation of the continuous casting billet comprises the following steps: Hot metal pretreatment - converter smelting - LF furnace refining - RH vacuum treatment - continuous casting; In the continuous casting process, the casting temperature of molten steel is ≤1540°C, and electromagnetic stirring or continuous casting billet light reduction process is adopted, and the billet light reduction rate is controlled at 5-7%.
3. The production method according to claim 2, characterized in that: The molten steel casting temperature is 1530~1540℃.
4. The production method according to claim 2, characterized in that: The molten iron pretreatment includes desulfurization and dephosphorization. The sulfur mass fraction of the molten iron is reduced to below 0.003%, and the phosphorus mass fraction is reduced to below 0.001%.
5. The production method according to claim 2, characterized in that: When smelting steel in converter, slag stopper balls are added to stop the slag.
Citation Information
Patent Citations
Anti-microbiological-corrosion steel plate for oil storage tank and manufacturing method for anti-microbiological-corrosion steel plate
CN113667891A
Two-heating-number rolling method for 1000 MPa grade hydroelectric steel plate
CN114134301A