A UV LED lamp bead
Through the mixing of silicone modified components and cured components, the problems of poor brittleness and UV resistance of existing UV LED lamp bead packaging materials are solved, and higher heat resistance and light transmission are achieved, and the packaging is improved. Overall performance of glue.
Patent Information
- Application Number
- CN202310879297.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-07-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-07-17
AI Technical Summary
The packaging materials of existing ultraviolet LED lamp beads such as epoxy resin and polyurethane glue have problems such as high brittleness, poor impact resistance and poor UV resistance, and it is difficult to meet the requirements of high light transmission and good heat dissipation performance.
Mixing silicone modified components and cured components at a weight ratio of 20-50:1 is used to prepare packaging glue with higher compatibility, improving the defects of traditional epoxy resins and polyurethane glues, and enhancing UV resistance, heat resistance and heat dissipation. performance and improve the light transmittance and toughness of the packaging glue through specific preparation methods.
It achieves better adhesive effect and compatibility with the UV LED lamp bead body, improves the UV resistance, heat resistance and light transmission of the packaging glue, and enhances its toughness and durability.
Smart Images

Figure CN116936716B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ultraviolet LED lamp beads, and in particular to an ultraviolet LED lamp bead. Background Art
[0002] As a special light source, UV LED lamp beads have a wide range of application prospects. Whether in anti-counterfeiting, medical beauty, plant growth, UV curing or environmental testing, UV LED lamp beads can play an important role. In order to obtain better stable output, UV LED requires a good heat dissipation environment or heat dissipation system. The existing UV LED lamp beads,
[0003] LED packaging refers to the packaging of light-emitting chips, which is quite different from integrated circuit packaging. The packaging of LEDs is not only required to protect the wick, but also to be able to transmit light. According to different application scenarios, different dimensions, heat dissipation solutions and luminous effects, LED packaging forms are divided into: pin type, power type packaging, surface mount type (SMD), chip-on-board direct mounting type (COB), Chip-LED, UVC metal, ceramic packaging, etc. Among them, LED packaging materials mainly include epoxy resin, polyurethane, silicone and other materials with high transparency, while the surface of polyurethane packaging glue is too soft, easy to bubble, and insufficiently cured, so it can only be used for potting of ordinary electrical components. The epoxy resin packaging glue that is currently used a lot also has defects such as high brittleness, poor impact resistance, low operating temperature, and poor UV resistance. Summary of the invention
[0004] In order to overcome the shortcomings and deficiencies in the prior art, an object of the present invention is to provide an ultraviolet LED lamp bead.
[0005] The purpose of the present invention is achieved through the following technical scheme: a UV LED lamp bead, comprising a UV LED lamp bead body and a packaging glue filled on the top of the UV LED lamp bead body, wherein the packaging glue is formed by mixing a silicone modified component and a curing component in a weight ratio of 20-50:1 and then curing.
[0006] The UV LED lamp beads of this invention use a packaging adhesive that is cured after mixing a silicone modified component and a curing component in a weight ratio of 20-50:1. The silicone modification has better compatibility and better bonding effect with the UV LED lamp bead body, and improves the defects of epoxy resin adhesive and polyurethane adhesive. It has stronger UV resistance, heat resistance and heat dissipation performance, better light transmittance and better toughness.
[0007] Preferably, the organosilicon modified component comprises the following raw materials in parts by weight:
[0008]
[0009] The curing component comprises the following raw materials in parts by weight:
[0010] 3-5 parts of curing agent
[0011] 1-2 parts of curing accelerator.
[0012] By adopting the above technical scheme, the organosilicon-modified component uses organosilicon-modified epoxy resin and organosilicon-modified polyurethane resin prepolymer as main raw materials, improves the light transmittance, heat resistance, UV resistance and mechanical properties of traditional epoxy resin and polyurethane, and is compounded with synergist, dispersant, antioxidant, defoaming agent and active diluent to synergistically enhance the effect. After the curing component and the organosilicon-modified component are mixed and cured, the compatibility of the encapsulation glue is further improved, the bonding effect with the ultraviolet LED lamp bead body is better, the ultraviolet resistance, heat resistance and heat dissipation performance are stronger, the light transmittance is better, and the toughness is better.
[0013] Preferably, the preparation method of each portion of the organosilicon-modified epoxy resin comprises the following steps:
[0014] (Q1), take 50-80 parts of bisphenol A epoxy resin, 10-20 parts of vinyl triethoxy silane, 100-120 parts of organic solvent and 1-5 parts of catalyst by weight, and set aside;
[0015] (Q2), taking bisphenol A epoxy resin and an organic solvent and mixing them evenly to obtain a mixed solution A;
[0016] (Q3) Under nitrogen conditions, the temperature was raised to 110°C, and vinyl triethoxysilane was added dropwise to the mixed solution A while stirring for 1 hour, and then a catalyst was added and reacted for 1-2 hours. After removing the catalyst, a silicone-modified epoxy resin was obtained.
[0017] By adopting the above technical scheme, bisphenol A epoxy resin is modified with vinyl triethoxy silane, which effectively improves the thermal stability, UV resistance and flexibility of the silicone-modified epoxy resin, and cooperates with the silicone-modified polyurethane resin prepolymer to achieve better overall thermal stability, UV resistance and flexibility.
[0018] More preferably, the bisphenol A epoxy resin is E-44, the organic solvent is a mixture of acetone and ethyl acetate in a weight ratio of 1:1; and the catalyst is boron trifluoride etherate.
[0019] Preferably, the preparation method of each portion of the organosilicon-modified polyurethane resin prepolymer comprises the following steps:
[0020] (R1), take 30-40 parts of polyether polyol, 80-100 parts of isophorone diisocyanate, 100-200 parts of solvent, 2-4 parts of chain extender and 8-12 parts of vinyl triethoxy silane by weight, and set aside;
[0021] (R2), mixing isophorone diisocyanate and a solvent to form a mixed solution B;
[0022] (R3), taking polyether polyol and removing water by vacuum, then heating to 80°C under nitrogen, adding the polyether polyol dropwise to the mixed solution B while stirring for 1-2 hours, then adding a chain extender and reacting at 70°C for 20-25 minutes to obtain a polyurethane prepolymer;
[0023] (R4), adding vinyl triethoxysilane to the polyurethane prepolymer, heating to 80-90° C. and stirring for 30-45 minutes to obtain a silicone-modified polyurethane resin prepolymer.
[0024] By adopting the above technical scheme, a polyurethane prepolymer is prepared mainly with polyether polyol and isophorone diisocyanate, and then reacted with vinyl triethoxysilane to obtain a silicone-modified polyurethane resin prepolymer, which has better heat resistance and UV resistance, and has a certain anti-foaming ability. It works synergistically with the defoamer to greatly increase the overall defoaming performance, reduce the amount of defoamer added, and effectively improve the light transmittance.
[0025] More preferably, the polyether polyol is at least one of polyoxypropylene polyol, polyoxyethylene polyol or polytetramethylene glycol, and the number average molecular weight is 1000-8000 g / mol; the solvent is isopropanol; and the chain extender is 1,4-butanediol.
[0026] Preferably, the synergist is prepared by mixing talc and fumed silica in a weight ratio of 3:1-2.
[0027] By adopting the above technical scheme, an appropriate amount of talcum powder and fumed silica are mixed and evenly distributed in the silicone modified component under the action of a dispersant, which has a significant synergistic effect on the overall light transmittance, smoothness, heat resistance and heat dissipation, tensile strength, toughness and anti-aging performance of the encapsulation glue.
[0028] More preferably, the dispersant is polyethylene glycol; and the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 4:1.
[0029] Preferably, the defoamer is organosilicon polysiloxane defoamer HY-6811; the active diluent is dodecyl glycidyl ether and / or 1,6-hexanediol diglycidyl ether.
[0030] Preferably, the curing agent is a mixture of an anhydride curing agent and a polyisocyanate curing agent in a weight ratio of 0.8:1-2; the curing accelerator is N,N-dimethylbenzylamine, triphenylphosphine or dodecylphenol. Further, the anhydride curing agent is maleic anhydride or phthalic anhydride, and the polyisocyanate curing agent is hexamethylene diisocyanate or 4,4'-diphenylmethane diisocyanate.
[0031] Furthermore, the preparation method of the packaging glue comprises the following steps:
[0032] A. Silicone modified components:
[0033] A1. Take organosilicon-modified epoxy resin, organosilicon-modified polyurethane resin prepolymer, synergist, dispersant, antioxidant, defoamer and reactive diluent by weight and set aside;
[0034] A2, taking a silicone-modified epoxy resin, a silicone-modified polyurethane resin prepolymer and a reactive diluent, and then adding a synergist, a dispersant, an antioxidant and a defoamer under stirring at room temperature to obtain a silicone-modified component;
[0035] B. Curing component: uniformly mix the curing agent and the curing accelerator according to parts by weight to obtain a curing component;
[0036] When in use, the organosilicon modified component and the curing component are mixed at a weight ratio of 20-50:1 and then filled on the top of the ultraviolet LED lamp bead body, and cured for 1 hour at 100-120° C. to obtain the encapsulation glue.
[0037] The preparation method of the encapsulation glue is simple to operate, convenient to control, high in production efficiency, low in production cost, and can be used for large-scale production.
[0038] The beneficial effects of the present invention are as follows: the packaging glue used in the ultraviolet LED lamp bead of the present invention is formed by mixing the organosilicon modified component and the curing component at a weight ratio of 20-50:1 and then curing, the organosilicon modified component has better compatibility and better bonding effect with the ultraviolet LED lamp bead body, and improves the defects of epoxy resin glue and polyurethane glue, has stronger ultraviolet resistance, heat resistance and heat dissipation performance, better light transmittance and better toughness. . BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a schematic diagram of the structure of the present invention;
[0040] The accompanying drawings are marked as follows: 1. UV LED lamp bead body; 2. Packaging glue. DETAILED DESCRIPTION
[0041] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments and drawings. The contents mentioned in the implementation modes are not intended to limit the present invention.
[0042] Example 1
[0043] like Figure 1 As shown, a UV LED lamp bead includes a UV LED lamp bead body and a packaging glue filled on the top of the UV LED lamp bead body, wherein the packaging glue is formed by mixing a silicone modified component and a curing component in a weight ratio of 35:1 and then curing.
[0044] The organosilicon modified component comprises the following raw materials in parts by weight:
[0045]
[0046] The curing component comprises the following raw materials in parts by weight:
[0047] 4 parts of curing agent
[0048] 1.5 parts of curing accelerator.
[0049] The preparation method of each portion of the organosilicon-modified epoxy resin comprises the following steps:
[0050] (Q1), take 65 parts of bisphenol A epoxy resin, 15 parts of vinyl triethoxy silane, 110 parts of organic solvent and 3 parts of catalyst by weight, and set aside;
[0051] (Q2), taking bisphenol A epoxy resin and an organic solvent and mixing them evenly to obtain a mixed solution A;
[0052] (Q3) Under nitrogen conditions, the temperature was raised to 110°C, and vinyl triethoxysilane was added dropwise to the mixed solution A while stirring for 1 hour. A catalyst was then added and the reaction was continued for 1.5 hours. After the catalyst was removed, a silicone-modified epoxy resin was obtained.
[0053] The bisphenol A epoxy resin is E-44, the organic solvent is a mixture of acetone and ethyl acetate in a weight ratio of 1:1; and the catalyst is boron trifluoride etherate.
[0054] The preparation method of each portion of the organosilicon-modified polyurethane resin prepolymer comprises the following steps:
[0055] (R1), take 35 parts of polyether polyol, 90 parts of isophorone diisocyanate, 150 parts of solvent, 3 parts of chain extender and 10 parts of vinyl triethoxy silane by weight, and set aside;
[0056] (R2), mixing isophorone diisocyanate and a solvent to form a mixed solution B;
[0057] (R3), taking polyether polyol and removing water by vacuum, then heating to 80°C under nitrogen, adding polyether polyol dropwise to mixed solution B while stirring for 1.5 hours, then adding chain extender and reacting at 70°C for 23 minutes to obtain polyurethane prepolymer;
[0058] (R4), adding vinyl triethoxysilane to the polyurethane prepolymer, heating to 85° C. and stirring for 35 minutes to obtain a silicone-modified polyurethane resin prepolymer.
[0059] The polyether polyol is polyethylene oxide polyol, and the number average molecular weight is 3000 g / mol; the solvent is isopropanol; and the chain extender is 1,4-butanediol.
[0060] The synergist is prepared by mixing talcum powder and fumed silicon dioxide in a weight ratio of 3:1.5.
[0061] The dispersant is polyethylene glycol; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 4:1.
[0062] The defoamer is organosilicon polysiloxane defoamer HY-6811; the active diluent is dodecyl glycidyl ether.
[0063] The curing agent is a mixture of maleic anhydride and hexamethylene diisocyanate in a weight ratio of 0.8:1.5; and the curing accelerator is N,N-dimethylbenzylamine.
[0064] The preparation method of the packaging glue comprises the following steps:
[0065] A. Silicone modified components:
[0066] A1. Take organosilicon-modified epoxy resin, organosilicon-modified polyurethane resin prepolymer, synergist, dispersant, antioxidant, defoamer and reactive diluent by weight and set aside;
[0067] A2, taking a silicone-modified epoxy resin, a silicone-modified polyurethane resin prepolymer and a reactive diluent, and then adding a synergist, a dispersant, an antioxidant and a defoamer under stirring at room temperature to obtain a silicone-modified component;
[0068] B. Curing component: uniformly mix the curing agent and the curing accelerator according to parts by weight to obtain a curing component;
[0069] When in use, the organosilicon modified component and the curing component are mixed according to a weight ratio and then filled on the top of the ultraviolet LED lamp bead body, and cured at 110° C. for 1 hour to obtain the encapsulation glue.
[0070] Example 2
[0071] like Figure 1As shown, a UV LED lamp bead includes a UV LED lamp bead body and a packaging glue filled on the top of the UV LED lamp bead body, wherein the packaging glue is formed by mixing a silicone modified component and a curing component in a weight ratio of 20:1 and then curing.
[0072] The organosilicon modified component comprises the following raw materials in parts by weight:
[0073]
[0074] The curing component comprises the following raw materials in parts by weight:
[0075] 3 parts of curing agent
[0076] 1 part of curing accelerator.
[0077] The preparation method of each portion of the organosilicon-modified epoxy resin comprises the following steps:
[0078] (Q1), take 50 parts of bisphenol A epoxy resin, 10 parts of vinyl triethoxy silane, 100 parts of organic solvent and 1 part of catalyst by weight, and set aside;
[0079] (Q2), taking bisphenol A epoxy resin and an organic solvent and mixing them evenly to obtain a mixed solution A;
[0080] (Q3) Under nitrogen conditions, the temperature was raised to 110°C, and vinyl triethoxysilane was added dropwise to the mixed solution A while stirring for 1 hour. A catalyst was then added and reacted for 1 hour. After removing the catalyst, a silicone-modified epoxy resin was obtained.
[0081] The bisphenol A epoxy resin is E-44, the organic solvent is a mixture of acetone and ethyl acetate in a weight ratio of 1:1; and the catalyst is boron trifluoride etherate.
[0082] The preparation method of each portion of the organosilicon-modified polyurethane resin prepolymer comprises the following steps:
[0083] (R1), take 30 parts of polyether polyol, 80 parts of isophorone diisocyanate, 100 parts of solvent, 2 parts of chain extender and 8 parts of vinyl triethoxy silane by weight, and set aside;
[0084] (R2), mixing isophorone diisocyanate and a solvent to form a mixed solution B;
[0085] (R3), taking polyether polyol and removing water by vacuum, then heating to 80°C under nitrogen, adding polyether polyol dropwise to mixed solution B while stirring for 1 hour, then adding chain extender and reacting at 70°C for 20 minutes to obtain polyurethane prepolymer;
[0086] (R4), adding vinyl triethoxysilane to the polyurethane prepolymer, heating to 80° C. and stirring for 30 minutes to obtain a silicone-modified polyurethane resin prepolymer.
[0087] The polyether polyol is polyethylene oxide polyol, and the number average molecular weight is 1000 g / mol; the solvent is isopropanol; and the chain extender is 1,4-butanediol.
[0088] The synergist is prepared by mixing talcum powder and fumed silicon dioxide in a weight ratio of 3:1.
[0089] The dispersant is polyethylene glycol; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 4:1.
[0090] The defoamer is organosilicon polysiloxane defoamer HY-6811; the active diluent is dodecyl glycidyl ether.
[0091] The curing agent is a mixture of maleic anhydride and hexamethylene diisocyanate in a weight ratio of 0.8:1; and the curing accelerator is dodecylphenol.
[0092] The preparation method of the packaging glue comprises the following steps:
[0093] A. Silicone modified components:
[0094] A1. Take organosilicon-modified epoxy resin, organosilicon-modified polyurethane resin prepolymer, synergist, dispersant, antioxidant, defoamer and reactive diluent by weight and set aside;
[0095] A2, taking a silicone-modified epoxy resin, a silicone-modified polyurethane resin prepolymer and a reactive diluent, and then adding a synergist, a dispersant, an antioxidant and a defoamer under stirring at room temperature to obtain a silicone-modified component;
[0096] B. Curing component: uniformly mix the curing agent and the curing accelerator according to parts by weight to obtain a curing component;
[0097] When in use, the organosilicon modified component and the curing component are mixed according to a weight ratio and then filled on the top of the ultraviolet LED lamp bead body, and cured at 110° C. for 1 hour to obtain the encapsulation glue.
[0098] Example 3
[0099] like Figure 1 As shown, a UV LED lamp bead includes a UV LED lamp bead body and a packaging glue filled on the top of the UV LED lamp bead body, wherein the packaging glue is formed by mixing an organic silicon modified component and a curing component in a weight ratio of 50:1 and then curing.
[0100] The organosilicon modified component comprises the following raw materials in parts by weight:
[0101]
[0102]
[0103] The curing component comprises the following raw materials in parts by weight:
[0104] 5 parts of curing agent
[0105] 2 parts of curing accelerator.
[0106] The preparation method of each portion of the organosilicon-modified epoxy resin comprises the following steps:
[0107] (Q1), take 80 parts of bisphenol A epoxy resin, 20 parts of vinyl triethoxy silane, 120 parts of organic solvent and 5 parts of catalyst by weight, and set aside;
[0108] (Q2), taking bisphenol A epoxy resin and an organic solvent and mixing them evenly to obtain a mixed solution A;
[0109] (Q3) Under nitrogen conditions, the temperature was raised to 110°C, and vinyl triethoxysilane was added dropwise to the mixed solution A while stirring for 1 hour. A catalyst was then added and reacted for 2 hours. After removing the catalyst, a silicone-modified epoxy resin was obtained.
[0110] The bisphenol A epoxy resin is E-44, the organic solvent is a mixture of acetone and ethyl acetate in a weight ratio of 1:1; and the catalyst is boron trifluoride etherate.
[0111] The preparation method of each portion of the organosilicon-modified polyurethane resin prepolymer comprises the following steps:
[0112] (R1), take 40 parts of polyether polyol, 100 parts of isophorone diisocyanate, 200 parts of solvent, 4 parts of chain extender and 12 parts of vinyl triethoxy silane by weight, and set aside;
[0113] (R2), mixing isophorone diisocyanate and a solvent to form a mixed solution B;
[0114] (R3), taking polyether polyol and removing water by vacuum, then heating to 80°C under nitrogen, adding polyether polyol dropwise to mixed solution B while stirring for 2 hours, then adding chain extender and reacting at 70°C for 25 minutes to obtain polyurethane prepolymer;
[0115] (R4), adding vinyl triethoxysilane to the polyurethane prepolymer, heating to 90° C. and stirring for 45 minutes to obtain a silicone-modified polyurethane resin prepolymer.
[0116] The polyether polyol is polyethylene oxide polyol, and the number average molecular weight is 8000 g / mol; the solvent is isopropanol; and the chain extender is 1,4-butanediol.
[0117] The synergist is prepared by mixing talcum powder and fumed silicon dioxide in a weight ratio of 3:2.
[0118] The dispersant is polyethylene glycol; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 4:1.
[0119] The defoamer is organosilicon polysiloxane defoamer HY-6811; the active diluent is dodecyl glycidyl ether.
[0120] The curing agent is a mixture of maleic anhydride and hexamethylene diisocyanate in a weight ratio of 0.8:2; and the curing accelerator is N,N-dimethylbenzylamine.
[0121] The preparation method of the packaging glue comprises the following steps:
[0122] A. Silicone modified components:
[0123] A1. Take organosilicon-modified epoxy resin, organosilicon-modified polyurethane resin prepolymer, synergist, dispersant, antioxidant, defoamer and reactive diluent by weight and set aside;
[0124] A2, taking a silicone-modified epoxy resin, a silicone-modified polyurethane resin prepolymer and a reactive diluent, and then adding a synergist, a dispersant, an antioxidant and a defoamer under stirring at room temperature to obtain a silicone-modified component;
[0125] B. Curing component: uniformly mix the curing agent and the curing accelerator according to parts by weight to obtain a curing component;
[0126] When in use, the organosilicon modified component and the curing component are mixed according to a weight ratio and then filled on the top of the ultraviolet LED lamp bead body, and cured at 110° C. for 1 hour to obtain the encapsulation glue.
[0127] Example 4
[0128] like Figure 1 As shown, a UV LED lamp bead includes a UV LED lamp bead body and a packaging glue filled on the top of the UV LED lamp bead body, wherein the packaging glue is formed by mixing a silicone modified component and a curing component in a weight ratio of 40:1 and then curing.
[0129] The organosilicon modified component comprises the following raw materials in parts by weight:
[0130]
[0131]
[0132] The curing component comprises the following raw materials in parts by weight:
[0133] 4 parts of curing agent
[0134] 1.2 parts of curing accelerator.
[0135] The preparation method of each portion of the organosilicon-modified epoxy resin comprises the following steps:
[0136] (Q1), take 70 parts of bisphenol A epoxy resin, 12 parts of vinyl triethoxy silane, 115 parts of organic solvent and 2 parts of catalyst by weight, and set aside;
[0137] (Q2), taking bisphenol A epoxy resin and an organic solvent and mixing them evenly to obtain a mixed solution A;
[0138] (Q3) Under nitrogen conditions, the temperature was raised to 110°C, and vinyl triethoxysilane was added dropwise to the mixed solution A while stirring for 1 hour. A catalyst was then added and the reaction was continued for 1.3 hours. After the catalyst was removed, a silicone-modified epoxy resin was obtained.
[0139] The bisphenol A epoxy resin is E-44, the organic solvent is a mixture of acetone and ethyl acetate in a weight ratio of 1:1; and the catalyst is boron trifluoride etherate.
[0140] The preparation method of each portion of the organosilicon-modified polyurethane resin prepolymer comprises the following steps:
[0141] (R1), take 33 parts of polyether polyol, 87 parts of isophorone diisocyanate, 150 parts of solvent, 3 parts of chain extender and 10 parts of vinyl triethoxy silane by weight, and set aside;
[0142] (R2), mixing isophorone diisocyanate and a solvent to form a mixed solution B;
[0143] (R3), taking polyether polyol and removing water by vacuum, then heating to 80°C under nitrogen, adding polyether polyol dropwise to mixed solution B while stirring for 1 hour, then adding chain extender and reacting at 70°C for 25 minutes to obtain polyurethane prepolymer;
[0144] (R4), adding vinyl triethoxysilane to the polyurethane prepolymer, heating to 90° C. and stirring for 30 minutes to obtain a silicone-modified polyurethane resin prepolymer.
[0145] The polyether polyol is polyethylene oxide polyol, and the number average molecular weight is 6000 g / mol; the solvent is isopropanol; and the chain extender is 1,4-butanediol.
[0146] The synergist is prepared by mixing talcum powder and fumed silicon dioxide in a weight ratio of 3:1.5.
[0147] The dispersant is polyethylene glycol; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 4:1.
[0148] The defoamer is organosilicon polysiloxane defoamer HY-6811; the active diluent is dodecyl glycidyl ether.
[0149] The curing agent is a mixture of maleic anhydride and hexamethylene diisocyanate in a weight ratio of 0.8:1.5; and the curing accelerator is N,N-dimethylbenzylamine.
[0150] The preparation method of the packaging glue comprises the following steps:
[0151] A. Silicone modified components:
[0152] A1. Take organosilicon-modified epoxy resin, organosilicon-modified polyurethane resin prepolymer, synergist, dispersant, antioxidant, defoamer and reactive diluent by weight and set aside;
[0153] A2, taking a silicone-modified epoxy resin, a silicone-modified polyurethane resin prepolymer and a reactive diluent, and then adding a synergist, a dispersant, an antioxidant and a defoamer under stirring at room temperature to obtain a silicone-modified component;
[0154] B. Curing component: uniformly mix the curing agent and the curing accelerator according to parts by weight to obtain a curing component;
[0155] When in use, the organosilicon modified component and the curing component are mixed according to a weight ratio and then filled on the top of the ultraviolet LED lamp bead body, and cured at 110° C. for 1 hour to obtain the encapsulation glue.
[0156] Comparative Example 1
[0157] The difference between this comparative example and Example 1 is:
[0158] The organosilicon-modified epoxy resin is directly replaced by bisphenol A epoxy resin E-44.
[0159] Comparative Example 2
[0160] The difference between this comparative example and Example 1 is:
[0161] The organosilicon-modified polyurethane resin prepolymer is replaced by a polyurethane prepolymer, and the preparation method of each portion of the polyurethane prepolymer comprises the following steps:
[0162] (R1), take 35 parts of polyether polyol, 90 parts of isophorone diisocyanate, 150 parts of solvent, 3 parts of chain extender and 10 parts of vinyl triethoxy silane by weight, and set aside;
[0163] (R2), mixing isophorone diisocyanate and a solvent to form a mixed solution B;
[0164] (R3), taking polyether polyol and removing water by vacuum, then heating to 80°C under nitrogen, adding polyether polyol dropwise to mixed solution B while stirring for 1.5 hours, then adding chain extender and reacting at 70°C for 23 minutes to obtain polyurethane prepolymer;
[0165] The polyether polyol is polyethylene oxide polyol, and the number average molecular weight is 3000 g / mol; the solvent is isopropanol; and the chain extender is 1,4-butanediol.
[0166] Comparative Example 3
[0167] The difference between this comparative example and Example 1 is:
[0168] The synergist is talcum powder.
[0169] Comparative Example 4
[0170] The difference between this comparative example and Example 1 is:
[0171] The synergist is fumed silica.
[0172] Comparative Example 5
[0173] The difference between this comparative example and Example 1 is:
[0174] The organosilicon modified component comprises the following raw materials in parts by weight:
[0175]
[0176] That is, the amount of enhancer in the packaging glue is 0 parts.
[0177] Comparative Example 6
[0178] The difference between this comparative example and Example 1 is:
[0179] The synergist is prepared by mixing talcum powder and titanium dioxide in a weight ratio of 3:1.5.
[0180] Comparative Example 7
[0181] The difference between this comparative example and Example 1 is:
[0182] The organosilicon modified component comprises the following raw materials in parts by weight:
[0183]
[0184] That is, the amount of the silicone-modified polyurethane resin prepolymer in the packaging glue is 0 parts.
[0185] Example 5
[0186] The encapsulation adhesives of Examples 1-4 and Comparative Examples 1-7 were cured and molded according to the test requirements, and the light transmittance and impact strength before and after light-heat aging were tested respectively.
[0187] Photothermal aging method: The cured sample was placed under UVA-340 lamp irradiation conditions at 25°C and 60°C, alternating between them every 2 hours for 30 days.
[0188] Light transmittance: The light transmittance of the cured sample (the encapsulation glue raw material is poured into a mold and molded into a 1 mm thick sheet) is tested using a spectrophotometer UV2600 at a wavelength of 560 nm.
[0189] Impact strength: According to GBT2567-2008 Test method for properties of resin castings, 5.4 simply supported beam impact toughness test, type I specimen, the impact strength is tested.
[0190] The test results are shown in Table 1:
[0191] Table 1
[0192]
[0193] As can be seen from Table 1 above, the encapsulation adhesive material used in the present invention, the organosilicon-modified component uses organosilicon-modified epoxy resin and organosilicon-modified polyurethane resin prepolymer as the main raw materials, improves the light transmittance, heat resistance and heat dissipation, UV resistance and mechanical properties of traditional epoxy resin and polyurethane, and adds synergist, dispersant, antioxidant, defoamer and active diluent compound, synergistic synergy, after the curing component and the organosilicon-modified component are mixed and cured, the compatibility of the encapsulation adhesive is further improved, and the bonding effect with the ultraviolet LED lamp bead body is better, the ultraviolet resistance, heat resistance and heat dissipation performance are stronger, the light transmittance is better, and the toughness is better. As can be seen from Examples 1-4, the light transmittance and heat resistance and UV resistance of the encapsulation adhesive of the present invention are more excellent, and the impact strength is greatly improved.
[0194] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A UV LED lamp bead, characterized in that: It includes an ultraviolet LED lamp bead body and a packaging glue filled on the top of the ultraviolet LED lamp bead body, wherein the packaging glue is formed by mixing an organic silicon modified component and a curing component at a weight ratio of 20-50:1 and then curing; The organosilicon modified component comprises the following raw materials in parts by weight: The curing component comprises the following raw materials in parts by weight: 3-5 parts of curing agent 1-2 parts of curing accelerator; The preparation method of each portion of the organosilicon-modified epoxy resin comprises the following steps: (Q1), take 50-80 parts of bisphenol A epoxy resin, 10-20 parts of vinyl triethoxy silane, 100-120 parts of organic solvent and 1-5 parts of catalyst by weight, and set aside; (Q2), taking bisphenol A epoxy resin and an organic solvent and mixing them evenly to obtain a mixed solution A; (Q3), under nitrogen conditions, the temperature was raised to 110°C, and vinyl triethoxysilane was added dropwise to the mixed solution A while stirring for 1 hour, and then a catalyst was added, and the reaction was continued for 1-2 hours. After removing the catalyst, an organosilicon-modified epoxy resin was obtained; The preparation method of each portion of the organosilicon-modified polyurethane resin prepolymer comprises the following steps: (R1), take 30-40 parts of polyether polyol, 80-100 parts of isophorone diisocyanate, 100-200 parts of solvent, 2-4 parts of chain extender and 8-12 parts of vinyl triethoxy silane by weight, and set aside; (R2), mixing isophorone diisocyanate and a solvent to form a mixed solution B; (R3), taking polyether polyol and removing water by vacuum, then heating to 80°C under nitrogen, adding the polyether polyol dropwise to the mixed solution B while stirring for 1-2 hours, then adding a chain extender and reacting at 70°C for 20-25 minutes to obtain a polyurethane prepolymer; (R4), adding vinyl triethoxysilane to the polyurethane prepolymer, heating to 80-90° C. and stirring for 30-45 minutes to obtain a silicone-modified polyurethane resin prepolymer; The synergist is prepared by mixing talcum powder and fumed silicon dioxide in a weight ratio of 3:1-2.
2. The ultraviolet LED lamp bead according to claim 1, characterized in that: The bisphenol A epoxy resin is E-44, the organic solvent is a mixture of acetone and ethyl acetate in a weight ratio of 1:1; and the catalyst is boron trifluoride etherate.
3. The ultraviolet LED lamp bead according to claim 1, characterized in that: The polyether polyol is at least one of polyoxypropylene polyol, polyoxyethylene polyol or polytetramethylene glycol, and the number average molecular weight is 1000-8000 g / mol; the solvent is isopropanol; and the chain extender is 1,4-butanediol.
4. The ultraviolet LED lamp bead according to claim 1, characterized in that: The dispersant is polyethylene glycol; the antioxidant is a mixture of antioxidant 1010 and antioxidant 168 in a weight ratio of 4:
1.
5. The ultraviolet LED lamp bead according to claim 1, characterized in that: The defoamer is an organosilicon polysiloxane defoamer HY-6811; the active diluent is dodecyl glycidyl ether and / or 1,6-hexanediol diglycidyl ether.
6. The ultraviolet LED lamp bead according to claim 1, characterized in that: The curing agent is a mixture of an anhydride curing agent and a polyisocyanate curing agent in a weight ratio of 0.8:1-2; the curing accelerator is N,N-dimethylbenzylamine, triphenylphosphine or dodecylphenol.