A method for regenerating waste chrome-aluminum bricks from steel smelting furnace
Through the steps of grinding, reduction, pickling and arc smelting, the performance degradation of waste chromium aluminum bricks due to iron oxide is solved, the efficient regeneration and utilization of chromium and aluminum elements and the improvement of material performance is achieved, and the chromium aluminum bricks are extended. Service life.
Patent Information
- Application Number
- CN202310705013.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-06-14
AI Technical Summary
The performance of waste chromium aluminum bricks in steel smelting furnaces has decreased due to long-term erosion and oxidation, and the existing reuse methods have led to a significant reduction in the value of elements and resource values.
By grinding waste chromium aluminum brick powder into 200 mesh fine powder and mixing it with coal powder, iron oxide is reduced in an atmosphere reduction furnace, and then pickling and smelting of the arc furnace to remove iron elements, improving the purity and crystalline properties of the chromium aluminum material. Form powders that can be used to regenerate chromium aluminum bricks.
The high-value reuse of chromium and aluminum elements in waste chromium aluminum bricks has been realized, the refractory performance and economic value of the material have been improved, and the service life of chromium aluminum bricks has been extended.
Abstract
Description
Technical Field
[0001] The invention relates to the field of secondary utilization of waste refractory materials, and in particular to a method for regenerating waste chrome-aluminum bricks of a steel smelting furnace. Background Art
[0002] Chrome aluminum bricks refer to bricks used in steel smelting furnaces. They are made of chrome aluminum crystal materials as raw materials, aluminum dihydrogen phosphate as a binder, pressed and formed by a press, and fired in a high-temperature shuttle kiln. They have high wear resistance and refractoriness. They also have good corrosion resistance to erosion and scouring by molten iron, molten steel, and non-ferrous metal solutions. They are widely used in the slide rails, steel tapping platforms, steel tapping troughs and other parts of heating furnaces. At present, it is found that this kind of bricks are gradually corroded by hot-rolled steel molten iron and surface oxide scale during long-term use, and cannot be used.
[0003] The waste chrome-aluminum bricks produced by the steel smelting furnace are subjected to the penetration and erosion of molten iron for a long time. The molten iron that penetrates in the high-temperature oxidation environment is oxidized and remains inside the chrome-aluminum bricks. As a result, the waste chrome-aluminum bricks contain a large amount of iron oxide, which will decompose at high temperatures to form ferroferric oxide and oxygen, resulting in vacancies or cracks in the waste chrome-aluminum bricks. At the same time, iron oxide is also magnetic, which seriously affects the refractory properties of the material. The general recycling method is to crush the chrome-aluminum bricks and use them as low-temperature refractory castable admixtures, which greatly reduces the element value and resource value. Summary of the invention
[0004] The present invention provides a method for regenerating waste chrome-aluminum bricks from a steel smelting furnace, so as to solve the deficiencies of the above-mentioned prior art and realize high-value recycling of chromium and aluminum element resources in the waste chrome-aluminum bricks from a steel smelting furnace.
[0005] In order to achieve the purpose of the present invention, the following technologies are proposed:
[0006] A method for regenerating waste chrome-aluminum bricks from a steel smelting furnace comprises the following steps:
[0007] Step 01, crushing and grinding the waste chrome-aluminum bricks to 200 mesh;
[0008] Step 02, mixing the waste chrome-aluminum brick powder obtained in step 01 with coal powder;
[0009] Step 03, placing the mixed powder obtained in step 02 in an atmosphere reduction furnace;
[0010] Step 04, acid washing the product obtained in step 03;
[0011] Step 05, drying the pickled material obtained in step 04;
[0012] Step 06, placing the material obtained in step 05 in an electric arc furnace for smelting, and cooling for 24 hours after smelting;
[0013] Step 07, dismantling, crushing and packaging the electric arc furnace in step 06 to obtain chromium-aluminum crystal material.
[0014] Furthermore, the fineness of the waste chrome-aluminum brick powder ground in step 01 is 200 mesh sieve residue ≤ 10%.
[0015] Furthermore, in the step 02, the fineness of the coal powder is 200 mesh and the residue is ≤10%.
[0016] Furthermore, the weight ratio of the waste chrome-aluminum brick powder to the coal powder in step 02 is 10:1-10:0.2.
[0017] Furthermore, in step 03, the reduction temperature in the atmosphere reduction furnace is 500°C-1300°C.
[0018] Furthermore, the acid used for pickling in step 04 is one or more of sulfuric acid, hydrochloric acid, and nitric acid, and the concentration of the acid is 0.5-10%.
[0019] Furthermore, in step 06, the electric arc furnace is a DC electric arc furnace or an AC electric arc furnace, and the smelting temperature is ≥ 2200°C.
[0020] Furthermore, the proportion of Cr2O3+Al2O3 in the waste chrome-aluminum bricks is ≥90%, and Fe2O3 is ≤5%.
[0021] Furthermore, in the chromium-aluminum material powder after pickling in step 05, the proportion of Cr2O3+Al2O3 is ≥95%, and the proportion of Fe2O3 is ≤0.3%.
[0022] Furthermore, in the chromium-aluminum crystal material in step 07, the proportion of Cr2O3+Al2O3 is ≥98%, and the proportion of Fe2O3 is ≤0.3%.
[0023] The advantages of the above technical solution are:
[0024] First, the present invention makes full use of the different redox properties of different oxides in waste chrome-aluminum bricks, and reduces the iron oxide therein to elemental iron that is easily acid-soluble in the atmosphere, while the chromium and aluminum elements are difficult to be reduced at low temperature, thereby achieving effective impurity removal of the chrome-aluminum material. The impurity-removed powder can be directly used to produce chrome-aluminum bricks, reducing the secondary grinding and iron increase of chrome-aluminum crystal materials. Secondly, the purified chrome-aluminum material powder is further melted to improve the crystal properties of the material, obtain chrome-aluminum crystal material, and greatly improve the economic value. The obtained chrome-aluminum material powder and chrome-aluminum crystal material particles are mixed in proportion to produce chrome-aluminum bricks for reuse in steel smelting furnaces. Chromium and aluminum resources are recycled with high value. DETAILED DESCRIPTION
[0025] Example 1
[0026] The waste chrome-aluminum bricks were ground into fine powders of ≤200 mesh. The content of Cr2O3, Al2O3 and Fe2O3 in the waste chrome-aluminum bricks were found to be 81.2%, 13.3% and 3.6% respectively. 100 kg of waste chrome-aluminum brick powder was weighed and mixed with 8.2 kg of 200-mesh coal powder. The mixture was placed in a steel belt atmosphere reduction furnace and heated to 800°C to reduce the iron oxide in the powder to elemental iron. The reduced powder was placed in a 0.5 m 3 The 2% hydrochloric acid solution was used for pickling; after pickling, 94.1 kg of low-iron chromium-aluminum material powder with a moisture content of 0.08% was obtained by drying, and the Cr2O3 content, Al2O3 content, and Fe2O3 content were 84.1%, 13.7%, and 0.14%, respectively; the powder was placed in an AC arc furnace for melting; after smelting, the furnace was dismantled and crushed to obtain chromium-aluminum crystal material particles, and the Cr2O3 content, Al2O3 content, and Fe2O3 content were 84.0%, 13.7%, and 0.16%, respectively, and the particles were packaged as products for export for the preparation of chrome-aluminum bricks.
[0027] Example 2
[0028] The waste chrome-aluminum bricks were ground into fine powders of ≤200 mesh. The content of Cr2O3, Al2O3 and Fe2O3 in the waste chrome-aluminum bricks were found to be 22.7%, 72.6% and 4.1% respectively. 100 kg of waste chrome-aluminum brick powder was weighed and mixed with 8.5 kg of 200-mesh coal powder. The mixture was placed in a steel belt atmosphere reduction furnace and heated to 1100°C to reduce the iron oxide in the powder to elemental iron. The reduced powder was placed in a 0.3 m 3 The chromium-aluminum crystalline material particles were packaged as products for export for the preparation of chromium-aluminum bricks.
[0029] Example 3
[0030] The waste chrome-aluminum bricks were ground into fine powders of ≤200 mesh. The content of Cr2O3, Al2O3 and Fe2O3 in the waste chrome-aluminum bricks were found to be 5.5%, 90.3% and 2.7% respectively. 100 kg of waste chrome-aluminum brick powder was weighed and mixed with 2.5 kg of 200-mesh coal powder. The mixture was placed in a push plate atmosphere reduction furnace and heated to 1050°C to reduce the iron oxide in the powder to elemental iron. The reduced powder was placed in a 0.3 m 3 The chromium-aluminum crystalline material particles were packaged and exported as products for the preparation of chromium-aluminum bricks.
[0031] Through the above-mentioned Examples 1-3, it is known that the Fe2O3 in the waste chrome-aluminum bricks can be effectively reduced and removed through the atmosphere reduction and pickling iron removal process, so it is known that the waste chrome-aluminum bricks of the steel smelting furnace can be recycled through the method proposed by the present invention, and greater economic benefits can be obtained. In addition, the chrome-aluminum material powder after iron removal is melted in an electric furnace to further produce chrome-aluminum crystal materials, which can be reused to produce chrome-aluminum bricks for steel smelting furnaces, realizing high-value recycling of resources.
[0032] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A method for regenerating waste chrome-aluminum bricks from steel smelting furnaces, characterized in that: Includes steps: Step 01, crushing and grinding the waste chrome-aluminum bricks to 200 meshes, wherein the proportion of Cr2O3+Al2O3 in the waste chrome-aluminum bricks is ≥90%, and the proportion of Fe2O3 is ≤5%; Step 02, mixing the waste chrome-aluminum brick powder obtained in step 01 with coal powder, wherein the weight ratio of the waste chrome-aluminum brick powder to the coal powder is 10:1-10:0.2; Step 03, placing the mixed powder obtained in step 02 in an atmosphere reduction furnace, wherein the reduction temperature in the atmosphere reduction furnace is 500° C.-1300° C.; Step 04, acid washing the product obtained in step 03; Step 05, drying the pickled material obtained in step 04, wherein the pickling acid is one or more of sulfuric acid, hydrochloric acid, and nitric acid, and the concentration of the acid is 0.5-10%; Step 06, placing the material obtained in step 05 in an electric arc furnace for smelting, and cooling for 24 hours after smelting. The electric arc furnace in step 06 is a DC electric arc furnace or an AC electric arc furnace, and the smelting temperature is ≥2200°C; Step 07, dismantling, crushing and packaging the electric arc furnace in step 06 to obtain chromium-aluminum crystal material, in which Cr2O3+Al2O3 accounts for ≥98%, and Fe2O3 accounts for ≤0.3%.
2. The method for regenerating waste chrome-aluminum bricks from steel smelting furnace according to claim 1, characterized in that: The fineness of the waste chrome-aluminum brick powder ground in step 01 is 200 mesh sieve residue ≤ 10%.
3. The method for regenerating waste chrome-aluminum bricks from steel smelting furnace according to claim 1, characterized in that: In the step 02, the coal powder fineness is 200 mesh and the residue is ≤10%.
4. The method for regenerating waste chrome-aluminum bricks from steel smelting furnace according to claim 1, characterized in that: In the chromium-aluminum material powder after pickling in step 05, the proportion of Cr2O3+Al2O3 is ≥95%, and the proportion of Fe2O3 is ≤0.3%.
Citation Information
Patent Citations
Method for smelting chromium metal from aluminum-chromium slag in electric arc furnace
CN105568004A
Method for producing iron alloy and refractory material by utilizing solid wastes
CN106673682A
Comprehensive utilization method for aluminum oxide red mud
CN107083485A
Method for regenerated production of chrome corundum by using waste high-chrome brick as raw material
CN107686343A
Method for producing ferrochrome and aluminum oxide by chrome-containing aluminum mud and red mud
CN109207736A