A highly corrosion-resistant coating for tundish lining
By using combined materials such as fused magnesia, magnesium oxide fine powder, and metal aluminum powder in the tundish coating, a high-density and low-pore coating is formed, which solves the problem of poor corrosion resistance in the existing technology and improves the performance of the tundish. Service life and hot strength.
Patent Information
- Application Number
- CN202310765747.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-06-26
AI Technical Summary
The existing tundish coating has poor corrosion resistance at high temperatures and high porosity, resulting in a short service life of the tundish. In addition, the phosphorus element in some formulas affects the quality of molten steel. It has good thermal insulation effect but insufficient corrosion resistance.
Using a combination of fused magnesia, magnesium oxide fine powder, metal aluminum powder, bonded clay, ρ-Al2O3, high-purity sodium lignosulfonate and SiO2 micro powder with a particle size of 0.1< to ≤3mm, the process is controlled to form a high-density, Low porosity coating uses metallic aluminum powder and ρ-Al2O3 to generate magnesia-aluminum spinel to enhance corrosion resistance.
Under the condition of ensuring that the flexural strength at room temperature is not less than 12.5MPa, the porosity is reduced to no more than 19.6%, the linear change rate at 1500℃ is -0.72~-1.0%, and the volume density is 2.30g/cm-3, which is improving. The service life of the package is at least 10% to enhance the corrosion resistance and hot strength of the coating.
Abstract
Description
Technical Field
[0001] The invention relates to a coating for steelmaking equipment, in particular to a coating for the inner lining of a steelmaking tundish. Background Art
[0002] The tundish is a continuous reactor. The quality of the tundish working lining directly determines the quality of the molten steel. The temperature of the tundish is about 1550℃, which determines the solidification point of the molten steel. The tundish should be loaded with molten steel that is several tens of degrees higher than 1550℃. In order to prevent the oxidation of the molten steel surface and reduce heat dissipation, protective slag is added. After the protective slag is heated by the molten steel, it will form an oxide melt on the steel surface and maintain this state until the casting is terminated. The tundish coating is a refractory working layer in direct contact with the molten steel. It must withstand long-term immersion and scouring of 1510-1580℃ molten steel and the erosion of the tundish slag. Therefore, the performance of the tundish coating determines the service life of the tundish, especially the slag line of the tundish, which needs to have higher corrosion resistance due to long-term contact with the molten body formed by the protective slag. Some of the tundish coatings currently used are constructed with a lot of water and have a large porosity. The molten steel and slag are easy to penetrate along the pores, which eventually leads to the peeling of the coating and the short service life of the tundish.
[0003] After searching:
[0004] The document with Chinese patent publication number CN103833394A discloses a "tundish coating" which uses magnesia as the main raw material and calcium lignin sulfonate and sodium tripolyphosphate as binders. Although this patented technology has the advantage of good thermal insulation performance, the introduction of phosphorus element has a certain impact on the quality of molten steel, and the good thermal insulation effect will lead to a large porosity, resulting in poor corrosion resistance and poor corrosion resistance.
[0005] The document with Chinese patent publication number CN104446565A discloses a "phosphorus-free and environmentally friendly tundish coating", which uses sintered magnesia, forsterite, paper fiber and liquid water glass or solid powdered water glass as raw materials. Although this patented technology has the advantages of being phosphorus-free and corrosion-resistant, too much water glass is added, and the Na2O contained in the water glass is easy to form low-melting products, which reduces the use temperature of the coating.
[0006] The Chinese patent publication number is CN 106518113 A, which discloses "A continuous casting tundish coating with good purification performance and its preparation method". By adding causticized white mud slag, the amount of water glass, explosion-proof fiber and high-aluminum cement added in the traditional coating formula is reduced, thereby reducing the cost by 5-10%. The addition of micro-nano-scale magnesium-aluminum hydrotalcite has a strong purification effect on molten steel; at the same time, by controlling the addition order in the coating preparation process, the performance and service life of the coating are guaranteed.
[0007] Another document discloses the effect of adding forsterite particles on the performance of magnesium tundish coating. It makes a magnesium tundish coating containing forsterite by adding 20% (w) of sintered or unsintered forsterite particles (3-1 mm), and studies the room temperature physical properties, slag erosion resistance and microstructure of the magnesium tundish coating containing forsterite particles. The results show that the volume density of the tundish coating with sintered forsterite particles is higher than that without forsterite particles, and the apparent porosity is reduced, and the room temperature flexural strength and compressive strength are slightly lower than those without forsterite particles; the volume density and strength of the coating with unsintered forsterite particles are slightly lower than those without forsterite particles; the static slag resistance test shows that the three tundish coatings are mainly eroded by penetration, regardless of whether they contain forsterite particles, and their slag erosion resistance is basically the same.
[0008] Metal aluminum powder can increase the density and hardness of refractory materials. It is generally used in magnesium carbon bricks and magnesium spinel bricks. It can be oxidized into aluminum oxide in the refractory material, or react with carbon to form aluminum carbide, or nitrided to form aluminum nitride. These substances are all high-temperature phases with high strength. They can also block pores, reduce porosity, and increase the density of the material. However, generally less aluminum powder is added. The main reason is that too much aluminum powder and too much spinel generated in situ with magnesium oxide in the material will cause the material to expand too much, which is prone to large cracks and pores. However, in the present invention, since a large amount of water is added in the construction process of the coating, the volatilization of water after baking will leave more gaps. At this time, adding an appropriate amount of aluminum powder will not cause the material to expand too much, but can fill the gaps and make the coating dense.
[0009] ρ-Al2O3 is a high-purity binder, generally used as a binder for high-purity amorphous refractory materials, such as a binder for corundum, alumina-spinel, aluminum-magnesium, mullite and other castables. Most of the aggregates of these castables are mainly aluminum oxide, so that no other elements will be introduced after the ρ-Al2O3 transforms into a crystalline phase at high temperature. In the present invention, the aggregate is mainly magnesium oxide, and ρ-Al2O3 will generate spinel with magnesium oxide at high temperature. The amount of metal aluminum powder and ρ-Al2O3 added is controlled, thereby controlling the content of spinel in the coating. Summary of the invention
[0010] The present invention aims to overcome the shortcomings of the prior art and provide a novel material which can reduce the porosity to no more than 19.6%, the linear change rate at 1500℃ to -0.72--1.0%, and the volume density to 2.30g / cm -3 , which can prolong the service life of the tundish by at least 10% compared with the original one by using a highly corrosion-resistant coating for the lining of the tundish.
[0011] Measures to achieve the above objectives:
[0012] A highly erosion-resistant coating for the inner lining of a tundish, the raw material composition and weight percentage content of which are: fused magnesia with a particle size of 0.1< to ≤3 mm: 50-65%, magnesium oxide fine powder with a particle size of ≤0.088 mm: 10-20%, metal aluminum powder: 3-9%, bonded clay with a particle size of ≤0.088 mm: 2-5%, ρ-Al2O3: 3-8%, sodium lignin sulfonate: 2-5%, SiO2 with a particle size of ≤0.015 mm: 1-4%;
[0013] In the fused magnesia with a particle size of 0.1< to ≤3 mm, the particle size of 1< to ≤3 mm accounts for 30-70%, and the particle size of 0.1< to ≤1 mm accounts for 30-70%.
[0014] The invention is that: the content of ρ-Al2O3% in the ρ-Al2O3 is not less than 80%, and the specific surface area is not less than 220m 2 g -1 .
[0015] Preferably, the weight percentage of the metal aluminum powder is 3.5-8.5%.
[0016] Preferably, the weight percentage content of ρ-Al2O3 is 3.5-6.5%.
[0017] Functions and mechanisms of various raw materials and main processes in the present invention
[0018] The reason why the present invention adds metallic aluminum powder and controls the content to 1-10%, preferably 3.5-8.5%, is that the metallic aluminum powder has the characteristics of being oxidized to generate aluminum oxide and in-situ generating magnesium aluminum spinel with magnesium oxide at high temperature. After fully utilizing its characteristics, the following are produced: first, a large amount of water is added to the middle package coating during the construction process, and voids are formed inside the coating after the water evaporates during baking. The melting point of metallic aluminum powder is about 660°C, and it can become a liquid phase during the middle package baking process, oxidized to generate aluminum oxide, and further reacted with magnesium sand to generate spinel. Both reactions have a certain volume expansion, which can effectively fill the voids formed by the volatilization of water during baking, promote the densification of the coating, and thus reduce the formation of cracks; second, the generated magnesium aluminum spinel can enhance the corrosion resistance of the coating.
[0019] The present invention adopts ρ-Al2O3 as a binder and sodium lignin sulfonate as a dispersant. Adding binding clay can play a role of plasticization and aiding binding. Adding SiO2 micropowder can enhance the medium-temperature strength of the coating (ρ-Al2O3 reacts with water to generate bayerite and boehmite gel to produce a binding effect, but the reaction is slow when the temperature is lower than 5°C. Adding sodium lignin sulfonate as a dispersant can accelerate the hydration reaction. In addition, ρ-Al2O3 dehydrates at medium temperature and is converted into α-Al2O3 at 1000°C. The medium-temperature strength of the coating will decrease. At this time, the added SiO2 micropowder and binding clay can increase the medium-temperature strength of the coating. At high temperature, ρ-Al2O3 can also form mullite with SiO2 or form magnesium spinel with magnesia, thereby enhancing the hot strength of the coating.
[0020] The metal aluminum powder and ρ-Al2O3 binder used in the present invention can eventually form magnesium spinel with the magnesia sand in the raw material, and do not bring in elements such as phosphorus and calcium contained in conventional coatings, thereby effectively improving the corrosion resistance of the coating.
[0021] Compared with the prior art, the present invention increases the porosity to no more than 19.6% while ensuring the room temperature flexural strength is no less than 12.5 MPa, the 1500°C linear change rate is -0.72 to -1.0%, and the volume density is 2.30 g / cm -3 The compressive strength at room temperature is not less than 72.5Mpa, and the hot flexural strength at 1500℃ is not less than 7.5MPa, so that the service life of the tundish can be increased by at least 10% compared with the original. DETAILED DESCRIPTION
[0022] The present invention is described in detail below:
[0023] Embodiment 1
[0024] A highly erosion-resistant coating for tundish lining, the raw material composition and weight percentage content of which are: fused magnesia with a particle size of 0.1< to ≤3 mm: 60%, magnesium oxide fine powder with a particle size of ≤0.088 mm: 16%, metal aluminum powder: 6%, bonded clay with a particle size of ≤0.088 mm: 5%, ρ-Al2O3: 6%, sodium lignin sulfonate: 5%, SiO2 with a particle size of ≤0.015 mm: 2%;
[0025] In the fused magnesia with a particle size of 0.1< to ≤3 mm, the particle size of 1< to ≤3 mm accounts for 60%, and the particle size of 0.1< to ≤1 mm accounts for 40%.
[0026] The above raw materials are the same as the conventional preparation process. After being coated on the inner wall of the tundish for trial use, the number of continuous casting furnaces of the tundish is increased by 15%. After testing, the room temperature flexural strength of this embodiment is 13.9MPa, the porosity is reduced to 17.6%, the linear change rate at 1500℃ is -0.81%, and the volume density is 2.48g / cm-3 The compressive strength at room temperature is 74.1Mpa, and the hot flexural strength at 1500℃ is 7.6MPa.
[0027] Embodiment 2
[0028] A highly erosion-resistant coating for tundish lining, the raw material composition and weight percentage content of which are: fused magnesia with a particle size of 0.1< to ≤3 mm: 65%, magnesium oxide fine powder with a particle size of ≤0.088 mm: 12%, metal aluminum powder: 5.5%, bonded clay with a particle size of ≤0.088 mm: 4.5%, ρ-Al2O3: 5.5%, sodium lignin sulfonate: 4.5%, SiO2 with a particle size of ≤0.015 mm: 3%;
[0029] In the fused magnesia with a particle size of 0.1< to ≤3 mm, the particle size of 1< to ≤3 mm accounts for 50%, and the particle size of 0.1< to ≤1 mm accounts for 50%.
[0030] The above raw materials are the same as the conventional preparation process. After being coated on the inner wall of the tundish for trial use, the number of continuous casting furnaces of the tundish is increased by 10%. After testing, the room temperature flexural strength of this embodiment is 13.4MPa, the porosity is reduced to 18.5%, the linear change rate at 1500℃ is -0.88%, and the volume density is 2.46g / cm -3 The room temperature compressive strength is 78.5Mpa, and the 1500℃ hot flexural strength is 7.9MPa.
[0031] Embodiment 3
[0032] A highly erosion-resistant coating for tundish lining, the raw material composition and weight percentage content of which are: fused magnesia with a particle size of 0.1< to ≤3 mm: 57%, magnesium oxide fine powder with a particle size of ≤0.088 mm: 18%, metal aluminum powder: 8%, bonded clay with a particle size of ≤0.088 mm: 4%, ρ-Al2O3: 5%, sodium lignin sulfonate: 4%, SiO2 with a particle size of ≤0.015 mm: 4%;
[0033] In the fused magnesia with a particle size of 0.1< to ≤3 mm, the particle size of 1< to ≤3 mm accounts for 55%, and the particle size of 0.1< to ≤1 mm accounts for 45%.
[0034] The above raw materials are the same as the conventional preparation process. After being coated on the inner wall of the tundish for trial use, the number of continuous casting furnaces of the tundish is increased by 10%. After testing, the room temperature flexural strength of this embodiment is 14.1MPa, the porosity is reduced to 18.2%, the linear change rate at 1500℃ is -0.79%, and the volume density is 2.50g / cm -3 The room temperature compressive strength is 73.2Mpa, and the 1500℃ hot flexural strength is 8.1MPa.
[0035] Embodiment 4
[0036] A highly erosion-resistant coating for tundish lining, the raw material composition and weight percentage content of which are: fused magnesia with a particle size of 0.1< to ≤3 mm: 53.5%, magnesium oxide fine powder with a particle size of ≤0.088 mm: 20%, metal aluminum powder: 9%, bonded clay with a particle size of ≤0.088 mm: 4.5%, ρ-Al2O3: 7%, sodium lignin sulfonate: 5%, SiO2 with a particle size of ≤0.015 mm: 1%;
[0037] In the fused magnesia with a particle size of 0.1< to ≤3 mm, the particle size of 1< to ≤3 mm accounts for 30%, and the particle size of 0.1< to ≤1 mm accounts for 70%.
[0038] The above raw materials are the same as the conventional preparation process. After being coated on the inner wall of the tundish for trial use, the number of continuous casting furnaces of the tundish is increased by 15%. After testing, the room temperature flexural strength of this embodiment is 15.8MPa, the porosity is reduced to 16.8%, the linear change rate at 1500℃ is -0.72%, and the volume density is 2.61g / cm -3 The room temperature compressive strength is 82.1Mpa, and the 1500℃ hot flexural strength is 9.2MPa.
[0039] Embodiment 5
[0040] A highly erosion-resistant coating for tundish lining, the raw material composition and weight percentage content of which are: fused magnesia with a particle size of 0.1< to ≤3 mm: 59%, magnesium oxide fine powder with a particle size of ≤0.088 mm: 20%, metal aluminum powder: 9%, bonded clay with a particle size of ≤0.088 mm: 3.5%, ρ-Al2O3: 3.5%, sodium lignin sulfonate: 2.5%, SiO2 with a particle size of ≤0.015 mm: 2.5%;
[0041] In the fused magnesia with a particle size of 0.1< to ≤3 mm, the particle size of 1< to ≤3 mm accounts for 60%, and the particle size of 0.1< to ≤1 mm accounts for 40%.
[0042] The above raw materials are the same as the conventional preparation process. After being coated on the inner wall of the tundish for trial use, the number of continuous casting furnaces of the tundish is increased by 10%. After testing, the room temperature flexural strength of this embodiment is 12.8MPa, the porosity is reduced to 19.6%, the linear change rate at 1500℃ is -0.98%, and the volume density is 2.33g / cm -3 The compressive strength at room temperature is 69.3Mpa, and the hot flexural strength at 1500℃ is 7.8MPa.
[0043] Embodiment 6
[0044] A highly erosion-resistant coating for tundish lining, the raw material composition and weight percentage content of which are: fused magnesia with a particle size of 0.1< to ≤3 mm: 63%, magnesium oxide fine powder with a particle size of ≤0.088 mm: 17%, metal aluminum powder: 7%, bonded clay with a particle size of ≤0.088 mm: 2.5%, ρ-Al2O3: 4%, sodium lignin sulfonate: 3.5%, SiO2 with a particle size of ≤0.015 mm: 3%;
[0045] In the fused magnesia with a particle size of 0.1< to ≤3 mm, the particle size of 1< to ≤3 mm accounts for 45%, and the particle size of 0.1< to ≤1 mm accounts for 55%.
[0046] The above raw materials are the same as the conventional preparation process. After being coated on the inner wall of the tundish for trial use, the number of continuous casting furnaces of the tundish is increased by 15%. After testing, the room temperature flexural strength of this embodiment is 13.2MPa, the porosity is reduced to 18.4%, the linear change rate at 1500℃ is -0.86%, and the volume density is 2.37g / cm -3 The room temperature compressive strength is 72.9Mpa, and the hot flexural strength at 1500℃ is 8.0MPa.
[0047] This specific implementation is only the best example and is not a restrictive implementation of the technical solution of the present invention.
Claims
1. A highly erosion-resistant coating for tundish lining, the raw material composition and weight percentage content of which are: fused magnesia with a particle size of 0.1< to ≤3 mm: 50-65%, magnesium oxide fine powder with a particle size of ≤0.088 mm: 10-20%, metallic aluminum powder: 3-9%, bonded clay with a particle size of ≤0.088 mm: 2-5%, ρ-Al2O3: 3-8%, sodium lignin sulfonate: 2-5%, SiO2 with a particle size of ≤0.015 mm: 1-4%; In the fused magnesia with a particle size of 0.1< to ≤3 mm, the particle size of 1< to ≤3 mm accounts for 30-70%, and the particle size of 0.1< to ≤1 mm accounts for 30-70%.
2. A highly corrosion resistant coating for tundish lining as claimed in claim 1, characterized in that: The content of ρ-Al2O3% in the ρ-Al2O3 is not less than 80%, and the specific surface area is not less than 220m 2 g -1 .
3. A highly corrosion resistant coating for tundish lining as claimed in claim 1, characterized in that: The weight percentage content of the metal aluminum powder is 3.5-8.5%.
4. A highly corrosion resistant coating for tundish lining as claimed in claim 1, characterized in that: The weight percentage of ρ-Al2O3 is 3.5-6.5%.
Citation Information
Patent Citations
Tundish coating
CN103833394A
Non-phosphorus environment-friendly tundish coating
CN104446565A
Continuous casting tundish paint with good purification function and preparation method thereof
CN106518113A
Carbon-free tundish coating material
CN110436893A
Magnesium-tundish phosphorus-free coating material
CN114836062A