A breathable and moisture permeable polyurethane coating for fabrics
By using modified graphene in fabric coating, the weather resistance and electrostatic problems of polyurethane materials are solved, the breathability, oxidation and antibacterial properties of the fabric are improved, and the overall performance and wear comfort of the fabric are improved.
Patent Information
- Application Number
- CN202310954950.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-01
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-08-01
AI Technical Summary
The polyurethane materials in existing fabric coatings have poor weather resistance, are prone to yellowing, and have insufficient electrostatic properties, which affects the comfort of wearing. They also produce static electricity after being combined with chemical fiber fabrics, affecting the use effect.
By grafting the long chain of organic molecules through chemical bonding, forming an organic layer, the modified graphene is uniformly dispersed in the polyurethane, improving water washing resistance and breathability, and introducing phosphite groups and quaternary ammonium salt functional groups. The pellets are used to enhance antioxidant and antistatic properties, and at the same time, they have a bactericidal effect by using the edges of graphene.
It significantly improves the moisture permeability, oxidation resistance, antistatic properties and antibacterial properties of the fabric, enhances the adhesion and mechanical properties of the coating, and improves the aging resistance and wear comfort of the fabric.
Smart Images

Figure SMS_1 
Figure SMS_3 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fabric coatings, and in particular relates to an air-permeable and moisture-permeable polyurethane coating for fabrics. Background Art
[0002] Fabric coating is an emerging industry that has developed rapidly in my country in the past decade. Coated fabrics are special materials with shielding functions that are made of various textiles as base fabrics and covered with chemical coating materials. Because coated fabrics not only have the original functions of fabrics, but also have the functions of covering layers, water-based polyurethane has good adhesion to various substrates, can give fabrics a soft and plump feel and leather feel, wear resistance, wrinkle resistance, shrinkage resistance, resilience, flexibility, breathability and moisture absorption, and the adjustment of polyurethane polymer structure can also be used for fabrics to be waterproof, oil-proof, anti-fouling, anti-pilling, etc., and can be used as fabric coatings, but polyurethane has poor weather resistance and is easy to yellow, causing fabric discoloration. At the same time, when combined with most chemical fiber fabrics, static electricity will be generated after friction, affecting wearing comfort. Therefore, under the premise of ensuring the excellent performance of polyurethane, it is of great practical significance to improve aging resistance, antistatic and other properties. Summary of the invention
[0003] The purpose of the present invention is to overcome the defects of the prior art and provide an air-permeable and moisture-permeable polyurethane coating for fabrics.
[0004] The invention grafts the long chain of organic molecules onto the graphene through chemical bonding to form an organic layer on the surface, which can promote the uniform dispersion of the modified graphene in the polyurethane and improve the water washing resistance of the organic molecules. The graphene itself has good moisture permeability and air permeability due to its tight forward stacking and high porosity. The phosphite group introduced by the modifier can capture free radicals to delay or inhibit oxidation reaction. The di-tert-butyl group provides a large steric hindrance to make it have good oxidation resistance. The graphene has good electrical conductivity. The grafted quaternary ammonium salt functional group can not only decomplex Positive and negative ions are generated for ion conduction, further improving the antistatic properties of coatings and fabrics. At the same time, it can be adsorbed on the surface of bacteria. The edges of graphene sheets are very sharp. When the cell membrane of bacteria contacts the edge of the sheet during activity, it will be scratched, causing the bacterial contents to flow out to achieve a bactericidal effect. The combination of the two has good antibacterial properties. The grafted -Si-O-Si- can be arranged in a directional and orderly manner to form a film on the surface of fabric fibers, making the fabric smooth and soft. The ester group can form hydrogen bonds with the -OH on the surface of cotton fibers, thereby improving the adhesion and mechanical properties of the coating.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A breathable and moisture-permeable polyurethane coating for fabrics, comprising the following raw materials in parts by weight: 80-100 parts of aqueous polyurethane emulsion, 4-6 parts of modified graphene, 0.1-0.2 parts of defoaming agent, 1-2 parts of polyurethane associative thickener, 0.1-0.2 parts of stabilizer, and 10-30 parts of deionized water;
[0007] The preparation method thereof comprises the following steps:
[0008] Aqueous polyurethane emulsion, deionized water, polyurethane associative thickener, defoamer, stabilizer and modified graphene are uniformly mixed, then coated on the surface of fabric, and then surface dried and cured to obtain an air-permeable and moisture-permeable polyurethane coating for fabric.
[0009] Furthermore, the defoaming agent is one or more of BYK1790, BYK067A and BYK085.
[0010] Furthermore, the stabilizer is one of triphenyl phosphate, trimethyl phosphate and trimethyl phosphite.
[0011] Furthermore, the modified graphene is prepared by the following steps:
[0012] S1. Place hydrogen-terminated silicone oil (molecular weight Mw=208g / mol) in a three-necked flask, add a platinum catalyst, stir and heat to 70°C, slowly drip dimethylallylamine dissolved in toluene into the flask, maintain the temperature for 2h, filter to remove the catalyst after the reaction, and then perform rotary evaporation to remove toluene from the reaction solution to obtain intermediate 1; the ratio of hydrogen-terminated silicone oil, platinum catalyst, dimethylallylamine, and toluene is 10g:0.14g:4.1g:40mL;
[0013] Under the catalytic action of platinum, hydrogen-terminated silicone oil and the unsaturated carbon-carbon double bond on the dimethylallylamine molecule undergo a hydrosilylation reaction to obtain intermediate 1. The specific reaction process is as follows:
[0014]
[0015] S2, intermediate 1 and chloroform are added to a three-necked flask, stirred for 5 minutes to completely dissolve, then chloroethyl isocyanate is added, the heating temperature is controlled to 65°C and refluxed for 10 hours. After the reaction is completed, chloroform is removed by vacuum rotary evaporation to obtain intermediate 2; the amount ratio of intermediate 1, chloroform and chloroethyl isocyanate is 10g:100mL:3.7g;
[0016] Under the action of chloroethyl isocyanate, the tertiary nitrogen on the intermediate 1 molecule undergoes a quaternization reaction to obtain intermediate 2. The specific reaction process is as follows:
[0017]
[0018] S3, toluene, tetra-n-butylammonium bromide and phosphorus trichloride were placed in a three-necked flask, 2,5-di-tert-butylphenol was slowly added dropwise at room temperature, the temperature was raised to 60°C after the addition was completed, and the reaction was stirred for 5 hours. After the reaction was completed, sodium carbonate aqueous solution was added to adjust the pH value to neutral, and then freeze-dried overnight. The product was recrystallized with isopropanol, and the crystallized product was washed three times with saturated brine, and then placed in a 50°C vacuum drying oven for 6 hours to obtain intermediate 3; the ratio of toluene, tetra-n-butylammonium bromide, phosphorus trichloride and 2,5-di-tert-butylphenol was 100mL:1g:8.5g:10g;
[0019] Under the catalysis of tetra-n-butylammonium bromide, -Cl on the phosphorus trichloride molecule reacts with -OH on the 2,5-di-tert-butylphenol molecule. Phosphorus oxychloride is volatile, so an excess of phosphorus oxychloride is added, and the reaction process shown below occurs to obtain intermediate 3;
[0020]
[0021] S4, triethylamine and intermediate 3 are placed in a three-necked flask, cyclohexane is added as a solvent, pentaerythritol is dissolved in cyclohexane, and slowly added dropwise to the three-necked flask at room temperature. After the addition is completed, the temperature is raised to 80°C, and the reaction is stirred for 5 hours. After the reaction is completed, the mixture is washed with 5% sodium bicarbonate solution and NaCl solution in sequence, and then vacuum evaporated. The product is recrystallized with isopropanol, and then placed in a 50°C vacuum drying oven for 6 hours to obtain intermediate 4; the ratio of cyclohexane, triethylamine, intermediate 3, and pentaerythritol is 100mL:1g:10g:4.4g;
[0022] Under the catalysis of triethylamine, -Cl on the intermediate 3 molecule reacts with -OH on the pentaerythritol molecule, and the molar ratio of the two is controlled to be 1:1, and the reaction process shown below occurs to obtain intermediate 4;
[0023]
[0024] S5, add intermediate 4 to a three-necked flask, add DMF as a solvent, stir for 5 minutes, heat to 50°C, then dissolve intermediate 2 in DMF, slowly dropwise add to the three-necked flask, then dropwise add dibutyltin dilaurate, maintain stirring at 50°C for 4 hours, after the reaction is completed, add ethyl acetate and deionized water, take the organic phase after layering, then wash it several times with a saturated NaCl solution, and finally perform reduced pressure rotary evaporation to obtain intermediate 5; the amount ratio of intermediate 4, intermediate 2, and dibutyltin dilaurate is 10g:7.8g:0.5mL;
[0025] Dibutyltin dilaurate is used as a catalyst, and the -OH on the intermediate 4 molecule reacts with the -NCO on the intermediate 2 molecule, and the molar ratio of the two is controlled to be close to 1:1 to obtain intermediate 5. The specific reaction process is as follows:
[0026]
[0027] S6. In a three-necked flask equipped with a thermometer, a condenser and a water separator, toluene, intermediate 5, p-toluenesulfonic acid and p-nitrophenylacetic acid were added in sequence. The heating temperature was controlled to be 115°C under nitrogen protection. The reaction was refluxed for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, a certain amount of distilled water was added, the organic phase was separated, and then washed with 5% sodium bicarbonate solution and NaCl solution in sequence, and then freeze-dried to obtain intermediate 6; the ratio of toluene, intermediate 5, p-toluenesulfonic acid and p-nitrophenylacetic acid was 100 mL: 10 g: 0.4 g: 2.5 g;
[0028] The molar ratio of intermediate 5 to p-nitrophenylacetic acid is controlled to be 1:1, and p-toluenesulfonic acid is used as a catalyst to cause an esterification reaction. The specific reaction process is as follows:
[0029]
[0030] S7, adding intermediate 6 and Raney nickel into a reaction kettle, adding 1,4-dioxane as a solvent, introducing nitrogen and hydrogen in turn for replacement, and then introducing hydrogen to a pressure of 3.7 MPa, reacting at 80°C for 7 hours, after the reaction is completed, filtering out the catalyst while hot, adding the filtrate into cold water, filtering out the precipitated solid, washing with water, and then vacuum drying to obtain a modifier; the amount ratio of intermediate 6, Raney nickel, and 1,4-dioxane is 10g:1.5g:100mL;
[0031] The nitro group on the middle 6 molecules is converted into amino group by Raney nickel catalysis and hydrogenation to obtain a modifier. The specific reaction process is as follows:
[0032]
[0033] S8, add the modifier, DMAP (N, N-dimethylaminopyridine) and DMF into a flask, then add EDC [N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride] and carboxylated graphene, introduce nitrogen protection, then ultrasonicate for 20 minutes, and then react at room temperature for 4 hours. After the reaction is completed, centrifuge the reaction solution, filter it, wash it with DMF and ethanol aqueous solution 2-3 times in turn, and finally put the product into a vacuum oven at 50°C to dry to obtain modified graphene; the ratio of the amount of modifier, DMAP, DMF, EDC, and carboxylated graphene is 10g:2g:100mL:3.2g:1g;
[0034] Under the action of DMAP and EDC, the -NH2 on the modifier molecule undergoes an amidation reaction with the -COOH grafted on the surface of the carboxylated graphene to obtain modified graphene.
[0035] Graphene is grafted with long chains of organic molecules through chemical bonding to form an organic layer on the surface, which can greatly improve the interfacial compatibility between modified graphene and polyurethane, thereby promoting the uniform dispersion of modified graphene in polyurethane and improving the water-washing resistance of organic molecules. Phosphite groups, tert-butyl groups, ester groups, quaternary ammonium salt structures, and -Si-O-Si- are introduced into the modified molecular chains. Graphene itself has good air permeability and can maintain high permeation vaporization efficiency due to its tight forward stacking and high porosity, making the coating have good moisture permeability and air permeability. The phosphite group can capture free radicals to delay or inhibit oxidation reactions. The di-tert-butyl group provides a large steric hindrance, which makes it have good antioxidant properties and can avoid discoloration of fabrics and coatings. Graphene has good electrical conductivity and is evenly distributed. After dispersion, the coating and fabric have good antistatic effect. The grafted quaternary ammonium salt functional groups can not only decomplex to generate positive and negative ions for ion conduction, further improving the antistatic properties of the coating and fabric, but also can be adsorbed on the surface of bacteria. The edges of the graphene sheets are very sharp. When the cell membrane of bacteria contacts the edge of the sheet during activity, it will be scratched, resulting in the outflow of bacterial contents to achieve the effect of sterilization. The combination of the two has good antibacterial properties. -Si-O-Si- has a high degree of rotational freedom and low interaction energy of methyl, so it has good film-forming properties on the surface of fabric fibers, can be arranged in a directional and orderly manner to form a film, reduce the surface tension of the fiber, make the fabric smooth and soft, and the ester group can form hydrogen bonds with the -OH on the surface of the cotton fiber, thereby improving the adhesion and mechanical properties of the coating.
[0036] Furthermore, the carboxylated graphene is prepared by the following steps:
[0037] Put graphene oxide and deionized water into a flask and disperse them ultrasonically for 1 hour to obtain a graphene oxide suspension; cool the suspension, add NaOH, and continue ultrasonication for 30 minutes; then add bromoacetic acid, disperse them ultrasonically for 15 minutes, and then react at room temperature for 5 hours. After the reaction, centrifuge the reaction solution, wash, filter, and vacuum dry to obtain carboxylated graphene powder; the ratio of graphene oxide, deionized water, NaOH, and bromoacetic acid is 100 mg: 100 mL: 1 g: 2 g.
[0038] Beneficial effects of the present invention:
[0039] The invention grafts the long chain of organic molecules onto the graphene through chemical bonding to form an organic layer on the surface, which can promote the uniform dispersion of the modified graphene in the polyurethane and improve the water washing resistance of the organic molecules. The graphene itself has good moisture permeability and air permeability due to its tight forward stacking and high porosity. The phosphite group introduced by the modifier can capture free radicals to delay or inhibit oxidation reaction. The di-tert-butyl group provides a large steric hindrance to make it have good oxidation resistance. The graphene has good electrical conductivity. The grafted quaternary ammonium salt functional group can not only decomplex Positive and negative ions are generated for ion conduction, further improving the antistatic properties of coatings and fabrics. At the same time, it can be adsorbed on the surface of bacteria. The edges of graphene sheets are very sharp. When the cell membrane of bacteria contacts the edge of the sheet during activity, it will be scratched, causing the bacterial contents to flow out to achieve a bactericidal effect. The combination of the two has good antibacterial properties. The grafted -Si-O-Si- can be arranged in a directional and orderly manner to form a film on the surface of fabric fibers, making the fabric smooth and soft. The ester group can form hydrogen bonds with the -OH on the surface of cotton fibers, thereby improving the adhesion and mechanical properties of the coating. DETAILED DESCRIPTION
[0040] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1
[0041] Preparation of carboxylated graphene:
[0042] 100 mg of graphene oxide and 100 mL of deionized water were placed in a flask and ultrasonically dispersed for 1 hour to obtain a graphene oxide suspension; the suspension was cooled, 1 g of NaOH was added, and ultrasonication was continued for 30 minutes; then 2 g of bromoacetic acid was added, ultrasonically dispersed for 15 minutes, and then reacted at room temperature for 5 hours. After the reaction, the reaction solution was centrifuged, washed, filtered, and vacuum dried to obtain carboxylated graphene powder. Example 2
[0043] Preparation of carboxylated graphene:
[0044] 200 mg of graphene oxide and 200 mL of deionized water were placed in a flask and ultrasonically dispersed for 1 hour to obtain a graphene oxide suspension; the suspension was cooled, 2 g of NaOH was added, and ultrasonication was continued for 30 minutes; then 4 g of bromoacetic acid was added, ultrasonically dispersed for 15 minutes, and then reacted at room temperature for 5 hours. After the reaction, the reaction solution was centrifuged, washed, filtered, and vacuum dried to obtain carboxylated graphene powder. Example 3
[0045] Preparation of modified graphene:
[0046] S1. Place 10 g of hydrogen-terminated silicone oil (molecular weight Mw = 208 g / mol) in a three-necked flask, add 0.14 g of platinum catalyst, stir and heat to 70°C, slowly drop 4.1 g of dimethylallylamine in 40 mL of toluene into the flask, maintain the temperature and react for 2 h. After the reaction is completed, filter to remove the catalyst, and then evaporate the reaction solution to remove toluene to obtain intermediate 1;
[0047] S2, add 10g of intermediate 1 and 100mL of chloroform into a three-necked flask, stir for 5min to completely dissolve it, then add 3.7g of chloroethyl isocyanate, control the heating temperature to 65°C and reflux for 10h, after the reaction is completed, remove chloroform by vacuum rotary evaporation to obtain intermediate 2;
[0048] S3, 100 mL of toluene, 1 g of tetra-n-butylammonium bromide and 8.5 g of phosphorus trichloride were placed in a three-necked flask, 10 g of 2,5-di-tert-butylphenol was slowly added dropwise at room temperature, the temperature was raised to 60°C after the addition was completed, and the reaction was stirred for 5 hours. After the reaction was completed, sodium carbonate aqueous solution was added to adjust the pH value to neutral, and then freeze-dried overnight. The product was recrystallized with isopropanol, and the crystallized product was washed three times with saturated brine, and then placed in a 50°C vacuum drying oven for 6 hours to obtain intermediate 3;
[0049] S4, 1g triethylamine and 10g intermediate 3 were placed in a three-necked flask, cyclohexane was added as a solvent, 4.4g pentaerythritol was dissolved in cyclohexane, and the mixture was slowly added dropwise to the three-necked flask at room temperature. After the addition was completed, the mixture was heated to 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate solution and NaCl solution in sequence, and then vacuum evaporated. The product was recrystallized with isopropanol, and then dried in a vacuum drying oven at 50°C for 6h to obtain intermediate 4;
[0050] S5, add 10g of intermediate 4 into a three-necked flask, add DMF as a solvent, stir for 5min, heat to 50°C, then dissolve 7.8g of intermediate 2 in DMF, slowly dropwise add into the three-necked flask, then dropwise add 0.5mL of dibutyltin dilaurate, keep stirring at 50°C for 4h, after the reaction is completed, add ethyl acetate and deionized water, take the organic phase after layering, then wash with saturated NaCl solution several times, and finally perform reduced pressure rotary evaporation to obtain intermediate 5;
[0051] S6. In a three-necked flask equipped with a thermometer, a condenser and a water separator, 100 mL of toluene, 10 g of intermediate 5, 0.4 g of p-toluenesulfonic acid and 2.5 g of p-nitrophenylacetic acid were added in sequence, the heating temperature was controlled to be 115°C under nitrogen protection, and the reaction was refluxed for 8 hours. After the reaction was completed, it was cooled to room temperature, a certain amount of distilled water was added, the organic phase was separated, and then washed with 5% sodium bicarbonate solution and NaCl solution in sequence, and then freeze-dried to obtain intermediate 6;
[0052] S7, add 10g of intermediate 6 and 1.5g of Raney nickel into a reaction kettle, add 100mL of 1,4-dioxane as a solvent, introduce nitrogen and hydrogen in sequence for replacement, then introduce hydrogen to a pressure of 3.7MPa, react at 80°C for 7h, after the reaction is completed, filter out the catalyst while hot, add the filtrate into cold water, filter out the precipitated solid, wash with water, and then vacuum dry to obtain a modifier;
[0053] S8. Add 10 g of modifier, 2 g of DMAP (N,N-dimethylaminopyridine) and 100 mL of DMF into a flask, then add 3.2 g of EDC [N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride] and 1 g of carboxylated graphene obtained in Example 1, introduce nitrogen protection, then ultrasonicate for 20 min, and then react at room temperature for 4 h. After the reaction, centrifuge the reaction solution, filter it, wash it with DMF and ethanol aqueous solution for 2-3 times in turn, and finally put the product into a vacuum oven at 50°C to obtain modified graphene. Example 4
[0054] Preparation of modified graphene:
[0055] S1. Place 20 g of hydrogen-terminated silicone oil (molecular weight Mw = 208 g / mol) in a three-necked flask, add 0.28 g of platinum catalyst, stir and heat to 70°C, slowly drop 8.2 g of dimethylallylamine in 80 mL of toluene into the flask, maintain the temperature and react for 2 h. After the reaction is completed, filter to remove the catalyst, and then evaporate the reaction solution to remove toluene to obtain intermediate 1;
[0056] S2, add 20g of intermediate 1 and 200mL of chloroform into a three-necked flask, stir for 5min to completely dissolve it, then add 7.4g of chloroethyl isocyanate, control the heating temperature to 65°C and reflux for 10h, after the reaction is completed, remove chloroform by vacuum rotary evaporation to obtain intermediate 2;
[0057] S3, 200 mL of toluene, 2 g of tetra-n-butylammonium bromide and 17 g of phosphorus trichloride were placed in a three-necked flask, 10 g of 2,5-di-tert-butylphenol was slowly added dropwise at room temperature, the temperature was raised to 60°C after the addition was completed, and the reaction was stirred for 5 hours. After the reaction was completed, sodium carbonate aqueous solution was added to adjust the pH value to neutral, and then freeze-dried overnight. The product was recrystallized with isopropanol, and the crystallized product was washed three times with saturated brine, and then placed in a 50°C vacuum drying oven for 6 hours to obtain intermediate 3;
[0058] S4, 2g of triethylamine and 20g of intermediate 3 were placed in a three-necked flask, cyclohexane was added as a solvent, 8.8g of pentaerythritol was dissolved in cyclohexane, and the mixture was slowly added dropwise to the three-necked flask at room temperature. After the addition was completed, the mixture was heated to 80°C and stirred for reaction for 5h. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate solution and NaCl solution in sequence, and then vacuum evaporated. The product was recrystallized with isopropanol, and then dried in a vacuum drying oven at 50°C for 6h to obtain intermediate 4;
[0059] S5, add 20g of intermediate 4 into a three-necked flask, add DMF as a solvent, stir for 5min, heat to 50°C, then dissolve 15.6g of intermediate 2 in DMF, slowly dropwise add into the three-necked flask, then dropwise add 1mL of dibutyltin dilaurate, keep stirring at 50°C for 4h, after the reaction is completed, add ethyl acetate and deionized water, take the organic phase after layering, then wash with saturated NaCl solution several times, and finally perform reduced pressure rotary evaporation to obtain intermediate 5;
[0060] S6. In a three-necked flask equipped with a thermometer, a condenser and a water separator, 200 mL of toluene, 20 g of intermediate 5, 0.8 g of p-toluenesulfonic acid and 5 g of p-nitrophenylacetic acid were added in sequence. The heating temperature was controlled to be 115°C under nitrogen protection. The reaction was refluxed for 8 hours. After the reaction was completed, it was cooled to room temperature. A certain amount of distilled water was added, and the organic phase was separated and then washed with 5% sodium bicarbonate solution and NaCl solution in sequence, and then freeze-dried to obtain intermediate 6.
[0061] S7, add 20g of intermediate 6 and 3g of Raney nickel into a reaction kettle, add 200mL of 1,4-dioxane as a solvent, introduce nitrogen and hydrogen in sequence for replacement, then introduce hydrogen to a pressure of 3.7MPa, react at 80°C for 7h, after the reaction is completed, filter out the catalyst while hot, add the filtrate into cold water, filter out the precipitated solid, wash with water, and then vacuum dry to obtain a modifier;
[0062] S8. Add 20 g of modifier, 4 g of DMAP (N,N-dimethylaminopyridine) and 200 mL of DMF into a flask, then add 6.4 g of EDC [N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride] and 2 g of carboxylated graphene obtained in Example 2, introduce nitrogen protection, then ultrasonicate for 20 min, and then react at room temperature for 4 h. After the reaction is completed, centrifuge the reaction solution, filter it, wash it with DMF and ethanol aqueous solution for 2-3 times in turn, and finally put the product into a vacuum oven at 50°C to obtain modified graphene. Example 5
[0063] 80 g of aqueous polyurethane emulsion, 10 g of deionized water, 1 g of polyurethane associative thickener, 0.1 g of BYK1790 defoamer, 0.1 g of triphenyl phosphate, and 4 g of modified graphene obtained in Example 3 were mixed evenly, then coated on the surface of the fabric, and then surface dried and cured to obtain a breathable and moisture-permeable polyurethane coating for fabric. Example 6
[0064] 90 g of aqueous polyurethane emulsion, 20 g of deionized water, 1.5 g of polyurethane associative thickener, 0.15 g of BYK067A defoamer, 0.15 g of trimethyl phosphate, and 5 g of modified graphene obtained in Example 4 were mixed evenly, then coated on the surface of the fabric, and then surface dried and cured to obtain a breathable and moisture-permeable polyurethane coating for fabric. Example 7
[0065] 100 g of aqueous polyurethane emulsion, 30 g of deionized water, 2 g of polyurethane associative thickener, 0.2 g of BYK085 defoamer, 0.2 g of trimethyl phosphite, and 6 g of modified graphene obtained in Example 3 were mixed evenly, then coated on the surface of the fabric, and then surface dried and cured to obtain a breathable and moisture-permeable polyurethane coating for fabric.
[0066] Comparative Example 1
[0067] Compared with Example 5, graphene is used instead of modified graphene in the preparation process, and the other raw materials and the preparation process remain unchanged, thereby obtaining a breathable and moisture-permeable polyurethane coating for fabric.
[0068] The air-permeable and moisture-permeable polyurethane coating for fabric obtained in Examples 5-7 and Comparative Example 1 was cut into pieces according to the standard and subjected to the following performance tests;
[0069] Implementation Standards Example 3 Example 4 Example 5 Comparative Example 2 Adhesion / Grade GB / T1720-79 1 1 1 2 Artificial aging resistance / 240h GB / T1865 No blistering, no peeling, no discoloration, level 1 No blistering, no peeling, no discoloration, level 1 No blistering, no peeling, no discoloration, level 1 No blistering, no shedding, no discoloration, level 2 Antibacterial rate GB / T20944.2-2007 92 90 93 88 <![CDATA[Surface charge density / uC·m -2 > GB / T12703.1-2008 0.071 0.075 0.079 0.92
[0070] It can be seen from the above table that the coating prepared in Control Example 1 has a lower adhesion level, and its anti-aging performance, antibacterial rate and charge surface density are all lower than those of Examples 5-7, indicating that Examples 5-7 prepared after graphene modification have better adhesion, anti-aging, antibacterial and antistatic properties.
[0071] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0072] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. A breathable and moisture permeable polyurethane coating for fabrics, It is characterized in that The invention comprises the following raw materials in parts by weight: 80-100 parts of aqueous polyurethane emulsion, 4-6 parts of modified graphene, 0.1-0.2 parts of defoaming agent, 1-2 parts of polyurethane associative thickener, 0.1-0.2 parts of stabilizer and 10-30 parts of deionized water; The modified graphene is prepared by the following steps: S1. Place hydrogen-terminated silicone oil in a three-necked flask, add a platinum catalyst, stir and heat to 70°C, slowly drip dimethylallylamine dissolved in toluene into the flask, maintain the temperature for 2 hours, filter to remove the catalyst after the reaction, and then perform rotary evaporation to remove toluene from the reaction solution to obtain intermediate 1; S2, add intermediate 1 and chloroform into a three-necked flask, stir for 5 minutes to completely dissolve, then add chloroethyl isocyanate, control the heating temperature to 65°C and reflux for 10 hours, after the reaction is completed, remove chloroform by vacuum rotary evaporation to obtain intermediate 2; S3, toluene, tetra-n-butylammonium bromide and phosphorus trichloride were placed in a three-necked flask, 2,5-di-tert-butylphenol was slowly added dropwise at room temperature, the temperature was raised to 60°C after the addition was completed, and the reaction was stirred for 5 hours. After the reaction was completed, sodium carbonate aqueous solution was added to adjust the pH value to neutral, and then freeze-dried overnight. The product was recrystallized with isopropanol, and the crystallized product was washed three times with saturated brine, and then placed in a 50°C vacuum drying oven for 6 hours to obtain intermediate 3; S4, triethylamine and intermediate 3 were placed in a three-necked flask, cyclohexane was added as a solvent, pentaerythritol was dissolved in cyclohexane, and the mixture was slowly added dropwise to the three-necked flask at room temperature. After the addition was completed, the mixture was heated to 80°C and stirred for reaction for 5 hours. After the reaction was completed, the mixture was washed with 5% sodium bicarbonate solution and NaCl solution in sequence, and then vacuum evaporated. The product was recrystallized with isopropanol, and then dried in a vacuum drying oven at 50°C for 6 hours to obtain intermediate 4; S5, add intermediate 4 to a three-necked flask, add DMF as a solvent, stir for 5 minutes, heat to 50°C, then dissolve intermediate 2 in DMF, slowly dropwise add to the three-necked flask, then dropwise add dibutyltin dilaurate, maintain stirring at 50°C for 4 hours, after the reaction is completed, add ethyl acetate and deionized water, take the organic phase after layering, then wash with saturated NaCl solution for several times, and finally perform reduced pressure rotary evaporation to obtain intermediate 5; S6. In a three-necked flask equipped with a thermometer, a condenser and a water separator, toluene, intermediate 5, p-toluenesulfonic acid and p-nitrophenylacetic acid were added in sequence, the heating temperature was controlled to be 115°C under nitrogen protection, and the reaction was refluxed for 8 hours. After the reaction was completed, the mixture was cooled to room temperature, a certain amount of distilled water was added, the organic phase was separated, and then washed with 5% sodium bicarbonate solution and NaCl solution in sequence, and then freeze-dried to obtain intermediate 6; S7, adding intermediate 6 and Raney nickel into a reaction kettle, adding 1,4-dioxane as a solvent, introducing nitrogen and hydrogen in sequence for replacement, and then introducing hydrogen to a pressure of 3.7 MPa, reacting at 80°C for 7 hours. After the reaction is completed, filtering out the catalyst while hot, adding the filtrate into cold water, filtering out the precipitated solid, washing with water, and then vacuum drying to obtain a modifier; S8. Add the modifier, N,N-dimethylaminopyridine and DMF into a flask, then add N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride and carboxylated graphene, introduce nitrogen protection, then ultrasonicate for 20 minutes, and then react at room temperature for 4 hours. After the reaction is completed, centrifuge the reaction solution, filter it, wash it with DMF and ethanol aqueous solution for 2-3 times in turn, and finally put the product into a vacuum oven at 50°C to dry to obtain modified graphene.
2. A breathable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that In step S1, the ratio of the amount of hydrogen-terminated silicone oil, platinum catalyst, dimethylallylamine, and toluene is 10 g: 0.14 g: 4.1 g: 40 mL.
3. The air-permeable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that In step S2, the usage ratio of intermediate 1, trichloromethane and chloroethyl isocyanate is 10 g:100 mL:3.7 g.
4. The air-permeable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that In step S3, the ratio of toluene, tetra-n-butylammonium bromide, phosphorus trichloride and 2,5-di-tert-butylphenol is 100 mL: 1 g: 8.5 g: 10 g.
5. The air-permeable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that In step S4, the ratio of cyclohexane, triethylamine, intermediate 3, and pentaerythritol is 100 mL: 1 g: 10 g: 4.4 g.
6. The air-permeable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that In step S5, the usage ratio of intermediate 4, intermediate 2, and dibutyltin dilaurate is 10 g:7.8 g:0.5 mL.
7. The air-permeable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that In step S6, the ratio of toluene, intermediate 5, p-toluenesulfonic acid, and p-nitrophenylacetic acid is 100 mL: 10 g: 0.4 g: 2.5 g.
8. The air-permeable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that In step S7, the usage ratio of intermediate 6, Raney nickel, and 1,4-dioxane is 10 g:1.5 g:100 mL.
9. The air-permeable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that In step S8, the ratio of the amount of the modifier, N,N-dimethylaminopyridine, DMF, N-(3-dimethylaminopropyl)-N'-ethylcarbodiimide hydrochloride, and carboxylated graphene is 10 g:2 g:100 mL:3.2 g:1 g.
10. The air-permeable and moisture-permeable polyurethane coating for fabric according to claim 1, It is characterized in that The defoaming agent is one or more of BYK1790, BYK067A and BYK085.